The invention relates to the field of thin film deposition, and, more particularly, to an apparatus and method for atomic layer deposition of films.
Atomic layer deposition (ALD) is a thin film deposition method that allows for the deposition of films having thicknesses on the order of nanometers in a precisely controlled way. Typically, ALD uses two or more gaseous precursors that are alternately and repeatedly applied to a substrate. A series of sequential steps in which a surface of the substrate is exposed to all precursors is called a deposition cycle. Each deposition cycle grows a single monolayer of film, or a fraction of a monolayer. This is due to the fact that, in ALD, film growth depends on chemisorption, a process whereby a precursor molecule adheres to a substrate's surface through the formation of a chemical bond (without further thermal decomposition of the precursor molecule taking place). Chemisorption stops naturally when all substrate surface sites available for chemical bonding with a precursor have been covered. Consequently, ALD is a self-limiting layer-by-layer deposition method that offers highly conformal coating and excellent thickness control. These characteristics make it a method of interest to various industries, among which in particular the semiconductor, and more specifically, the solar cell industry.
In the solar cell industry, ALD may be used to deposit aluminum oxide (Al2O3) films for the passivation of advanced mono-Si solar cells. To this end typical film thicknesses of 5-15 nm are required, which can be achieved using traditional single or multi-wafer ALD systems. Currently, the throughput of the most efficient multi-wafer ALD systems at said film thickness is about 60 wafers per hour. The amount of surface area to be treated in order to obtain—for example—a solar cell panel for use on a rooftop, is considerable however. And with the demand for solar cell panels on the rise, there is an increasing need for ALD apparatus featuring a higher throughput. Of course, the solar cell industry is exemplary only, and merely one of many industries in which the continual pressure for ALD equipment having an increased throughput is felt.
Such higher throughput is preferably achieved using apparatus that are relatively simple from a constructional point of view. This is because, typically, the simpler an apparatus is, the more economically it may be built, the more reliable it is and the less servicing it requires. It is therefore an object of the present invention to provide a device and a method for atomic layer deposition offering an improved throughput capacity at a minimum level of constructional complexity.
According to one aspect of the invention, an atomic layer deposition apparatus is provided. The apparatus includes a process tunnel that extends in a transport direction and that is bounded by at least a first, lower wall and a second, upper wall. Said walls are mutually parallel and spaced apart so as to allow a substantially flat substrate, oriented parallel to the walls, to be accommodated there between. The apparatus further includes a plurality of gas injection channels. These gas injection channels are provided in both the first wall and the second wall of the process tunnel and are disposed in a spaced apart manner along the transport direction. The gas injection channels in the first, lower wall are configured to provide a first, lower gas bearing, while the gas injection channels in the second, upper wall are configured to provide a second, upper gas bearing. The gas bearings are configured to floatingly support and accommodate substrates. Viewed in the transport direction, gas injection channels in at least one of the first wall and the second wall are connected successively to a first precursor gas source, a purge gas source, a second precursor gas source and a purge gas source, so as to create a tunnel segment that—in use—comprises successive zones including a first precursor gas, a purge gas, a second precursor gas and a purge gas, respectively. Two or more of such tunnel segments are disposed in succession in the transport direction. Viewed in the transport direction, at least a portion of the process tunnel has a downward slope (α), so as to enable gravity driven transport of substrates through said at least one process tunnel portion.
According to an aspect of the invention, a method is provided for growing a film on a substrate. The method comprises providing a first, lower gas bearing and a second, upper gas bearing, said gas bearings being configured to floatingly support and accommodate the substrate between them. The gas bearings extend downwards in a longitudinal transport direction. The method also comprises providing a substrate, and supporting and accommodating it between the gas bearings. The method further comprises enabling gravity to convey the substrate along the gas bearings in the transport direction, while subjecting a surface of the substrate to an atomic layer deposition treatment.
According to an aspect of the method according to the invention, at least one of the first and second gas bearings, viewed in the transport direction, is divided into two or more functional segments, each segment comprising at least four laterally extending zones that successively include a first precursor gas, a purge gas, a second precursor gas and a purge gas, respectively, and an atomic layer is deposited onto at least one surface of the substrate as it is conveyed through all at least four zones of a single functional segment of said gas bearing.
These and other features and advantages of the invention will be more fully understood from the following detailed description of certain embodiments of the invention, taken together with the accompanying drawings, which are meant to illustrate and not to limit the invention.
The disclosed atomic layer deposition apparatus includes a process tunnel through which a substrate, preferably as part of a train of substrates, may be conveyed in a linear manner. That is, the substrate may be inserted into the tunnel at an entrance thereof to be conveyed to an exit. The tunnel is bounded by at least two substantially parallel tunnel walls. These tunnel walls are located close to both the substrate and each other, so as to provide an elongate processing space with a relatively small volume per unit of length. In its longitudinal direction, the process tunnel is divided into a series of segments. In use each segment comprises a number—typically four—of laterally extending gas zones. Successive zones within a segment comprise a first precursor gas, a purge gas, a second precursor gas, and a purge gas respectively. As the substrate moves through the tunnel, its surface (e.g. its lower surface, its upper surface, or both) is strip-wise subjected to contact with the different gases. Provided the arrangement of the zones and the respective gases are chosen properly, traversal of one tunnel segment may be equivalent to subjecting the substrate to one atomic layer deposition cycle. Since the tunnel may comprise as many segments as desired, a film of arbitrary thickness may be grown on a substrate during its crossing through the tunnel. The linear nature of the process tunnel enables a continuous stream of substrates to be processed, thus delivering an atomic layer deposition apparatus with an appreciably improved throughput capacity.
To convey a substrate in the transport direction, the process tunnel is fitted with two gas bearings, located opposite each other and capable of receiving a substrate between them. A lower bearing supports the substrate from below, while an upper bearing covers substrate from above, thereby pressing it against the lower gas bearing so as to flatten it, and stabilize its position. The lower gas bearing may be provided for via the gas injection channels that are disposed in the lower, first tunnel wall, while the upper gas bearing may be provided for via the gas injection channels that are disposed in the upper, second tunnel wall. As the process tunnel slopes downwards, so do the tunnel walls and the gas bearings provided therein. Consequently, a substrate accommodated by the gas bearings will experience a gravitational force (component) that pulls it in the transport direction. This gravitational force causes the substrate to advance glidingly through the process tunnel. The presently disclosed apparatus thus features a substrate drive mechanism that is essentially passive in that substrates are gravity driven. Such a ‘gravity drive’ eliminates the need for a separate substrate conveyor whose parts are subject to soiling (due to their continuous traversal of the deposition environment maintained in the process tunnel), wear and inevitable periodic servicing, and as a result enables a simpler, more economical and more reliable ALD apparatus design.
From here on, reference is made to the appended drawings. In these drawings, identical reference numbers identify similar elements or acts. The sizes and relative positions of elements in the drawings are not necessarily drawn to scale. The shapes of various elements and angles may, for example, not be drawn to scale, and some of these elements may have been arbitrarily enlarged and positioned to improve drawing legibility. Further, the particular shapes of the elements as drawn are not intended to convey any information regarding the actual shape of the particular elements, and may have been selected solely for ease of recognition in the drawings.
Both tunnel walls 110, 120 are fitted with a plurality of gas injection channels 112 and 122, respectively. The outflow openings of the gas injection channels 112, 122 are distributed over the inside surfaces of the respective tunnel walls 110, 120 that are facing the substrate, both along the lateral and the longitudinal directions thereof. In
The gas injection channels 112, 122 in the tunnel walls 110, 120 are connected to (a number of) gas sources 114 and 124, respectively. Gas injection channels in the same tunnel wall and at the same longitudinal position thereof (e.g. the gas injection channels 112 visible in
In use, the gas injection channels 112, 122 may inject gases into the tunnel space 102 over the whole length of the tunnel. Once injected, the gases flow laterally between the tunnel walls 110, 120. When a substrate 130 is present, this means that the gases flow laterally across the lower and upper surfaces 130a, 130b of the substrate 130, towards the edges of the substrate and beyond. Lateral gas flows occur provided that the gases can escape at both lateral sides of the tunnel. To this end, the side walls 106 of the process tunnel may be provided with exhaust channels 108. An exhaust channel 108 is preferably held at or around atmospheric pressure, so as to render vacuum pumps superfluous. Alternatively, however, an exhaust channel 108 may be held at a pressure that deviates from atmospheric pressure, such as a lower or higher pressure. The sidewalls 106 restrict the outflow of gas. They stagnate the lateral gas flows and cause pressure buildup in the tunnel space regions 103 adjacent the side walls 106, which helps to stabilize the lateral position of the floating substrate 130.
It is understood that the gas injection channels 112 in the lower, first wall 110 generally provide for the lateral gas streams that occupy the lower half of the process tunnel space 102 (i.e. the lower gas bearing 113), whereas the gas injection channels 122 in the upper, second wall 120 generally provide for the lateral gas streams that occupy the upper half of the process tunnel space (i.e. the upper gas bearing 123). When a substrate 130 is present between both tunnel walls 110, 120, the lateral gas streams in the lower half of the process tunnel space 102 serve as the gas bearing that floatingly supports the substrate from below.
In
Attention is now invited to the manner in which substrates 130 may be conveyed through the process tunnel. As discussed above, the atomic layer deposition apparatus according to the present invention relies, at least in part, on the force of gravity to transport substrates through the process tunnel. This ‘gravity drive’ requires the process tunnel to slope downwards as shown in
Referring to
The net force on the substrate 130 in the direction of the process tunnel, denoted Fn, is assumed to be the resultant of two opposing forces: a viscous drag force acting on the bottom and top surfaces 130a, 130b of the substrate, denoted Fd, and a component of the force of gravity pulling the substrate through the process tunnel, denoted Fg,x, such that
F
n
=F
g,x
−F
d (1)
The viscous drag force Fd, which results from the interaction between the surfaces 130a, 130b of the substrate 130 and the gas bearings 113, 123, respectively, may be expressed as
wherein Δu/Δy denotes a velocity gradient in each of the gas bearings, present on both sides of the substrate (between the substrate's surfaces 130a, 130b and the respective tunnel walls 110, 120), η denotes a viscosity of the gas bearings, 2A denotes the combined surface area of the bottom and top surfaces of the substrate, vs denotes the velocity of the substrate in the transport direction of the process tunnel, and dg denotes the gap or distance between the bottom and top surfaces of the substrate and the first and second tunnel wall, respectively. In practice, the viscosity η may be approximated by a weighted average of the viscosities of the used purge and precursor gases, taking into account the relative lengths of the respective zones as weighting factors.
The gravitational force Fg,x pulling the substrate 130 in the transport direction 104 may be expressed as
F
g,x
=m·g·sin(α)=ρ·V·g·sin(α)=ρ·ds·A·g·sin(α) (3)
wherein m denotes the mass of the substrate, g denotes the gravitational acceleration, α denotes the angle of inclination of the process tunnel relative to the horizontal, ρ denotes the density of the substrate, V denotes the volume of the substrate, and ds denotes the thickness of the substrate.
Combining equations (1), (2) and (3), and setting the net force Fn to zero, yields the following expression for the equilibrium velocity of the substrate vs,eq
The equilibrium velocity as expressed by equation (4) is the velocity that a substrate 130 will ultimately assume after it has been inserted into the process tunnel. The equilibrium velocity vs,eq establishes itself as follows. Once the substrate 130 is in the process tunnel, it will experience a slope-related gravitational pull Fg,x in the transport direction 104. The gas bearings 113, 123, in turn, induce an oppositely directed speed-dependent drag Fd on the substrate 130: the greater the speed of the substrate (relative to the speed of the gas bearings in the transport direction), the greater the drag force, see equation (2). When the pull of gravity exceeds the drag, the substrate speeds up, and vice versa. A net force Fn pulling on the substrate 130 thus causes the drag on the substrate to increase until the drag force Fd equals the gravitational force Fg,x, from which point on the substrate's speed remains constant at vs,eq. Likewise, a net force Fn dragging on the substrate will cause the substrate 130 to slow down until the drag force Fd equals the gravitational force Fg,x and the substrate assumes a constant velocity vs,eq.
The time it takes a substrate 130 to acquire the equilibrium speed vs,eq depends on its initial velocity, i.e. the velocity at which it is inserted into the process tunnel. The time constant τ of the first-order differential equation in vs
which is a compilation of Newton's second law and equations (1), (2) and (3), is
Assuming a zero initial velocity, it will take the substrate approximately 5τ to acquire (over 99% of) its equilibrium velocity vs. In this time period, an inserted substrate will travel a distance xeq of
An important conclusion that may be drawn from equation (4) is that the equilibrium velocity vs,eq of a substrate 130 is dependent not only on the angle of inclination α of the process tunnel, but also on the product of the substrate thickness ds and the gap width dg. The angle of inclination α, and the spacing between the lower and upper tunnel walls (i.e. the height of the process tunnel) H are design parameters that can be accurately chosen. In the real world, there may be significant variations in thickness around a target thickness among substrates. Such thickness variations may result in variations in the product dsdg and, hence, in variations in the equilibrium velocity vs,eq, which is undesirable as it may result in collisions between substrates. Given that
H=d
s+2dg (8)
it follows that
from which it may be inferred that, at a given value of H, the product of substrate thickness ds and gap width dg has a maximum at
H=2 ds (10)
Thus, everything else being equal, a maximum equilibrium substrate velocity vs,eq may be obtained by choosing a height H such that it equals about twice the specified substrate thickness ds which implies that the gap width dg equals approximately half the substrate thickness ds. The advantage of this choice is that relatively small variations of the substrate thickness ds and corresponding variations in the gap width dg around their target values, have only a marginal impact on the value of their product as a larger substrate thickness is (practically completely) compensated for by a reduced gap width, and vice versa. In other words, the variations in forward gravitational force and in the drag force as a result of variations in substrate thickness are substantially equal and compensate each other. Configurations wherein H falls within the range 1.4 ds≦H≦5.0 ds may be considered to obey equation (10) to sufficient approximation for most practical purposes. More preferably H falls within the range 1.8 ds≦H≦2.2 ds.
Equation (10) may be implemented both statically and dynamically in an atomic layer deposition apparatus 100. In a static implementation, the embodiment of the atomic layer deposition apparatus 100 features a process tunnel with a fixed tunnel height H that is chosen in relation to one typical substrate thickness ds of substrates to be processed. In a dynamic implementation, the spacing H between the first tunnel wall 110 and the second tunnel wall 120 is adaptable upon changes of the typical substrate thickness ds. This allows the performance of the atomic layer deposition apparatus 100 to be optimized for batches of substrates 130 having mutually varying thicknesses. A dynamic implementation may therefore include a spacing adjuster or spacing adaptation means, e.g. in the form of a distributed, possibly motor driven high precision jack mechanism, for changing the spacing H between the first wall 110 and the second wall 120 over at least a portion of the process tunnel.
In an alternative embodiment it was found that a gap width dg of about 150 μm results in gas bearing characteristics that are sufficiently “stiff”, which means that the gas bearings 113, 123 keep the substrates in a stable position, spaced from the lower and upper walls of the tunnel while allowing movement in a direction parallel to the lower and upper walls. For lower values of dg, the design becomes very critical and for higher values of dg the gas bearing becomes rather soft. For practical purposes dg may preferably have a value between 100 μm and 1 mm. For the height H it means that H may preferably be in a range between (ds+100 μm) and (ds+2 mm), and more preferably that H has a value in a range between (ds+200 μm) and (ds (ds+400 μm) even if this means that equation (10) is not met, or H is not in the range 1.4 ds≦H≦5.0 ds. Typical substrate thicknesses lie in the range of 50 μm to 1000 μm.
As regards the angle of inclination α, it is noted that the slope of the process tunnel is preferably determined in relation to at least the minimum time periods that a substrate 130 must be exposed to the gases in each of the respective reactive gas zones 202, 204. There is no need for the slope of the process tunnel to be constant along its entire length. In a mixed ALD apparatus, for example, wherein different tunnel segments 208 comprise different gases having mutually different viscosities, a process tunnel having a locally varying slope α may be advantageous. A smaller slope α may for example be employed to offset a locally smaller viscosity η, and vice versa, so as to maintain an approximately constant substrate speed throughout the process tunnel.
In order to allow an atomic layer deposition apparatus 100 to be used in combination with substrates of different material densities ρ, and/or with gases having different viscosities η, it may be provided with a tilt adjuster configured to enable changing of the slope α of at least a portion of the process tunnel. Changing substrates 130 for more dense ones, for example, may require the slope α of the process tunnel to be reduced in order to ensure that the denser substrates are still exposed sufficiently long to the reactive gases in the respective gas zones. Likewise, changing precursors for ones having a higher viscosity η may require the slope α of the process tunnel to be increased. A tilt adjuster or tilt adjustment mechanism may have any suitable form, and may typically include pivotal arrangement of the process tunnel to allow for easy manipulation of its slope.
In some embodiments of the disclosed atomic layer deposition apparatus 100, the above-discussed passive gravity drive may be supplemented by other, auxiliary drive and/or guide systems.
One such auxiliary drive system is illustrated in
Another auxiliary drive system may include grooves in the tunnel walls 110, 120, the grooves being elongated in the longitudinal direction and having one end proximate a gas injection channel 112, 122 or a gas exhaust channel, as disclosed in U.S. Pat. No. 6,824,619 of applicant, which is incorporated herein by reference, where it is used to impart a rotational movement on a floating substrate. Similarly, this method can be used to impart linear movement to a substrate.
As the quality of a deposited film may depend on the surface temperature of the substrate during processing, substrates may be preheated before being subjected to the deposition process. Preheating of a substrate may be done by providing the deposition apparatus with a special pre-heat tunnel segment, located upstream of the first reactive tunnel segment, i.e. the first tunnel segment wherein a substrate is subjected to two or more precursors. In the pre-heat tunnel segment, a substrate may be brought into contact with no more than a purge gas, which is kept at the same or at a higher temperature than that of the reactive sections. Similarly, a cool-down segment may be provided at the end of the process tunnel, downstream of the last reactive tunnel segment. As the primary purpose of the purge gas in the pre-heat and cool-down segments is to transfer heat, helium—which has a relatively high thermal conductivity—is a good choice that helps to minimize the length of such a segment. In one embodiment of the atomic layer deposition apparatus, a pre-heat and/or cool-down segment may additionally serve to allow substrates to speed up or slow down. Such double function segments may for example be equipped with slanted gas injection channels as described with reference to
Further, to facilitate the loading and discharging of substrates into/from the process tunnel by a mechanical substrate handler, an entrance and/or an exit segment of the tunnel—reactive or non-reactive—may be provided with a larger spacing H between the tunnel walls to increase the gap dg between the upper 130b and lower 130a surface of an inserted substrate 130 and the upper 120 and lower 110 tunnel wall, respectively. A larger gap dg between the tunnel walls 110, 120 and the substrate 130 comes at the penalty of an increased gas flow rate, since the force to be delivered by the lower gas bearing to carry the weight of the substrate does not change.
Entrance section 300 is shown schematically in a lateral cross-sectional view in
The substrate handler 302 may release a substrate 130 with zero initial velocity. Alternatively, the substrate handler 302 may impart some forward momentum to the substrate 130 as is releases it. In a preferred embodiment, the substrate handler 302 is configured to feed substrates 130 at a speed smaller than an equilibrium speed that the substrates obtain when moving through the process tunnel, so as to reduce the chance of collisions between consecutively inserted substrates.
The dimensions and working parameters of the disclosed atomic layer deposition apparatus may vary, depending on the specific application it is built and used for. Here is an illustrative example in some numeric detail. Depositing a 10 nm film of aluminum oxide onto a standard circular 300 mm silicon wafer may involve two precursors, tri-methyl aluminum (Al(CH3)3, TMA) and water (H2O). As an alternative for water, ozone (O3) may be used. Nitrogen (N2) may be used both as an inert carrier gas in the precursor zones and as purge gas in the purge gas zones. Each of the zones may have a length of several centimeters, typically 2-5 cm, in the transport direction. To accommodate a single train of wafers, each having a lateral dimension of 300 mm, the width of the process tunnel needs to measure a little over 300 mm. In case a precursor zone measures 5 cm in length, whereas a purge gas zone measures 2 cm, the length of a single tunnel segment amounts to 0.14 m. As a single tunnel segment is responsible for depositing one monolayer of aluminum oxide of about 0.1 nm thickness, a total of 100 segments is required to grow a 10 nm film. Consequently, the length of the process tunnel needed for deposition comes to approximately 14 meters. Wafers may be transported through the tunnel at a speed as high as 0.25 m/s, which, for this specific example, would lead to a throughput capacity of about 3000 wafers per hour. Using the following estimates: ρ≈2300 kgm−3, ds≈200 μm, g=9.81 ms−2, η=2.5·10−5 kgm−1s−1, and abiding by equation (10), equation (4) yields a desired angle of inclination α of approximately 1.6°. In case the initial speed of the wafers is not equal to the desired equilibrium speed of 0.25 m/s, the process tunnel may have to be extended so as to provide for an entrance portion wherein the wafers can speed up or slow down to their desired equilibrium velocities. Substituting the above numbers into equation (6) results in τ=0.92. Substituting this value into equation (7), together with vs,eq=0.25 m/s, such an entrance portion would have to measure about 0.92 m in length in case the substrates have zero initial velocity.
Above, the invention has been described in terms of a first and a second precursor. One skilled in the art will recognize, however, that atomic layer deposition may be performed using more than two precursors. It is emphasized here, that the language of the claims does not intend to exclude an atomic layer deposition apparatus featuring three, four or more precursors. To that end, each segment may comprise three, four or more precursor gas injection zones all separated by purge gas injection zones. The segments of a process tunnel need not be identical. Nanolaminate films may for example be deposited when a number of successive segments of a first configuration for depositing a number of monolayers of a first film having a first composition, is alternated by a number of successive segments of a second configuration, for depositing a number of monolayers of a second film having a second composition. And such a sequence of segments can be repeated until the desired number of nanofilms is deposited. Also, although only aluminum oxide was mentioned specifically as an example of a material film to be deposited, it will be clear that the apparatus and method of the invention can be applied in combination with all precursor materials and film compositions that are now known in the art.
In addition, it is noted that the substrate may have a circular form, a square form, a rectangular form or triangular form or any other form that is available. Preferably, the form of the substrate is such that it allows a good filling of a surface area when the substrates are placed adjacent to each other, such as a square or rectangular form. Another general measure that may be taken to increase the throughput capacity of the ALD apparatus is to widen the process tunnel, so as to enable it to accommodate two or more parallel trains of substrates. Doubling the width of the tunnel, for example, potentially doubles the throughput of the apparatus.
Further, while illustrative embodiments of the present invention have been described above, in part with reference to the accompanying drawings, it is to be understood that the invention is not limited to these embodiments. Variations to the disclosed embodiments can be understood and effected by those skilled in the art in practicing the claimed invention, from a study of the drawings, the disclosure, and the appended claims. Reference throughout this specification to “one embodiment” or “an embodiment” means that a particular feature, structure or characteristic described in connection with the embodiment is included in at least one embodiment of the present invention. Thus, the appearances of the phrases “in one embodiment” or “in an embodiment” in various places throughout this specification are not necessarily all referring to the same embodiment. Particular features, structures, or characteristics of one or more embodiments may be combined in any suitable manner to form new, not explicitly described embodiments.
| Filing Document | Filing Date | Country | Kind | 371c Date |
|---|---|---|---|---|
| PCT/NL2009/050270 | 5/20/2009 | WO | 00 | 1/6/2011 |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 12123745 | May 2008 | US |
| Child | 12993361 | US |