The present invention relates to an apparatus for plasma atomic layer deposition for forming a thin film on a substrate.
The atomic layer deposition method, in which gases of elements constituting a thin film to be formed are alternately supplied onto a substrate to form a thin film in units of atomic layers on the substrate, is known as a technique for uniformly forming a thin film. Compared with a common CVD (Chemical Vapor Deposition) method, the atomic layer deposition method excels in step covering property and film thickness controllability.
Repeating the formation of a thin film by the atomic layer deposition method will lead to adhesion of the thin film even on an inner surface of a film forming chamber. As the thickness of the thin film adhered to the inner surface of the film forming chamber increases, the deposited thin film will be peeled off and part of the thin film becomes particles, causing deterioration of the quality of the thin film formed on the substrate. For that reason, it is preferable to remove the thin film deposited on the inner surface of the film forming chamber at regular intervals.
Patent Literature 1 proposes a processing method and apparatus in which an anti-adhesion plate is used and besides deposits deposited on the inner wall of a chamber are covered with an amorphous film in a vapor-phase growing apparatus for CVD film forming, sputter film forming, and the like. Although it is possible to reduce the frequency of cleaning by such means in a conventional vapor-phase growing apparatus, when the thickness of the deposits deposited on the inner wall of the chamber and the amorphous film covering the deposits becomes not less than a predetermined thickness, it is necessary to perform cleaning by using a wet etching method. However, in the wet etching method, since the film forming chamber is opened up, the time and effort for the opening work increases as the size of the film forming chamber increases, and therefore, when a gas etching method can be used, it is preferable to use the gas etching method. To perform etching by the gas etching method, while it is necessary to heat a portion of the inner wall surface of the film forming chamber, onto which a thin film has adhered, to a temperature not less than a predetermined temperature, a portion apart from the heater may not reach a necessary heating temperature, making it difficult to perform gas etching. For that reason, if a certain amount of thin film has adhered to a location where it is difficult to perform gas etching, it becomes necessary to open up the film forming chamber and perform wet etching.
There is proposed a technique for inserting an anti-adhesion plate in a film forming chamber for the purpose of increasing the interval of wet etching, and further suppressing film adhesion to the film forming chamber body (Patent Literature 2). In a conventional scheme, the anti-adhesion plate is divided to be placed in the film forming chamber. Dividing the anti-adhesion plate makes the handling thereof easy, and further, in the case of an apparatus for heating to higher temperatures, it becomes possible to absorb thermal expansion of the anti-adhesion plate by providing space in gaps between divided anti-adhesion plates.
However, in an apparatus for atomic layer deposition, a raw material gas and a reaction gas will readily infiltrate into fine gaps, forming films. Gases that have filtrated into such fine gaps turn into film and powder, thus causing particles. Therefore, in an apparatus for atomic layer deposition, it is preferable to suppress the dividing of the anti-adhesion plate as much as possible.
To suppress film adhesion in a case in which the dividing of anti-adhesion plate is needed, it is possible to employ a method of supplying inert gas as shown, for example, in Patent Literature 3.
Moreover, in an atomic layer deposition without use of plasma, it is possible to protect an upper part of the substrate by employing the anti-adhesion plate shown in Patent Literature 4. On the other hand, in a parallel-plate type plasma apparatus, in which an electrode for applying high-frequency voltage to an upper section of the substrate is placed, an insulator is used for supporting the electrode to which high-frequency voltage is applied. For this insulator, mainly, resins such as Teflon (registered trademark), and ceramics are used.
[Patent Literature 1] Japanese Patent Laid-Open No. 2006-351655
[Patent Literature 2] Japanese Patent Laid-Open No. 2009-62579
[Patent Literature 3] Japanese Patent Laid-Open No. 2012-52221
[Patent Literature 4] Japanese Patent Laid-Open No. 2012-126977
However, although an insulating support which fixes an upper electrode can be reproduced by wet etching, there is a risk that as a result of disassembling the support and reconstructing the plate electrode, the mounting position of the plate electrode is shifted from a previous mounting position, and thereby the plasma condition is changed from that before maintenance. Therefore, it is not preferable to perform maintenance of the insulating support, and the insulating support is preferably maintenance free.
Accordingly, it is conceivable to utilize an insulating anti-adhesion plate for the insulating support. In that occasion, the insulating anti-adhesion plate is fixed by fixing means such as a screw. However, since film adhesion readily occurs even in a screw hole in atomic layer deposition, the screw is firmly fixed by the force of film. Therefore, once film adhesion occurs, large force is required to remove the screw, and in such an occasion, the screw and the anti-adhesion plate are likely to be broken if they are made of a ceramic. Since resins may possibly be deformed, they are difficult to use.
Thus, since the maintenance of the insulating support becomes also complicated when an anti-adhesion plate is used, it is preferable to suppress any possible film adhesion on this portion.
It is an objective of the present invention to provide an apparatus for plasma atomic layer deposition which is capable of reducing the frequency of cleaning the film forming chamber and adhesion preventive members within the film forming chamber, and reducing the number of maintenance parts, thus improving maintenance workability.
That is, a first embodiment of the apparatus for plasma atomic layer deposition of the present invention is an apparatus for plasma atomic layer deposition for forming a thin film on a substrate, comprising:
a film forming chamber;
a plate electrode provided so as to face a substrate retained in the film forming chamber;
a counter electrode retaining the substrate within the film forming chamber;
a gas-introducing opening section provided in one side wall section of the film forming chamber; and an exhaust opening section provided in the other side wall section, which faces the one side wall section, of the film forming chamber, wherein
the apparatus for plasma atomic layer deposition further comprises:
an insulating injector adhesion preventive member which is mountable to the gas-introducing opening section from inside the film forming chamber, and is disposed in a tubular shape so as to surround an opening of the gas-introducing opening section;
an insulating exhaust adhesion preventive member which is mountable to the exhaust opening section from inside the film forming chamber, and is disposed in a tubular shape so as to surround an opening of the exhaust opening section; and
an insulating film forming chamber adhesion preventive member which is mountable to an inner wall side of the film forming chamber, wherein
the injector adhesion preventive member is separated from each of the plate electrode and the counter electrode side by a gap, and is configured such that its tip end is located inside with reference to the plate electrode end on the gas-introducing opening section side,
the exhaust adhesion preventive member is separated from each of the plate electrode and the counter electrode side by a gap, and is configured such that its tip end is located inside with reference to the plate electrode end on the exhaust opening section side, and
the film forming chamber adhesion preventive member is located at least on each side of the injector adhesion preventive member and the exhaust adhesion preventive member and to be separated from each of the plate electrode and the counter electrode side by a gap; and
the apparatus for plasma atomic layer deposition further comprises
an upper inert-gas supply port that purges inert gas toward inside the film forming chamber from the gap between the plate electrode, and each of the injector adhesion preventive member, the exhaust adhesion preventive member, and the film forming chamber adhesion preventive member;
a lower inert-gas supply port that purges inert gas toward inside the film forming chamber from the gap between the counter electrode, and each of the injector adhesion preventive member, the exhaust adhesion preventive member, and the film forming chamber adhesion preventive member;
an upper inert-gas supply section to be connected to the upper inert-gas supply port; and
a lower inert-gas supply section to be connected to the lower inert-gas supply port.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the injector adhesion preventive member extends such that its tip end position is located in a range of not less than 0.1 mm to not more than 200 mm from the plate electrode end toward the plate electrode center, with reference to the plate electrode end on the gas-introducing opening section side, and
the exhaust adhesion preventive member extends such that its tip end position is located in a range of not less than 0.1 mm to not more than 200 mm from the plate electrode end toward the plate electrode center, with reference to the plate electrode end on the exhaust opening section side.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
a side end section of a tubular opening section by the injector adhesion preventive member has a distance of not less than 0.1 mm and not more than 200 mm outwardly from the end section on the sideward side of the substrate retained by the counter electrode, and
a side end section of a tubular opening section by the exhaust adhesion preventive member has a distance of not less than 0.1 mm and not more than 200 mm outwardly from the end section on the sideward side of the substrate retained by the counter electrode.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the film forming chamber adhesion preventive member has a size to cover a vertical width of a side section of the injector adhesion preventive member and a side section of the exhaust adhesion preventive member, and an inner side surface of the film forming chamber adhesion preventive member and an outer side surface of the injector adhesion preventive member have a gap of not less than 0.1 mm and not more than 20 mm in horizontal distance therebetween, and an inner side surface of the film forming chamber adhesion preventive member and an outer side surface of the exhaust adhesion preventive member have a gap of not less than 0.1 mm and not more than 20 mm in horizontal distance therebetween.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the film forming chamber adhesion preventive member and the injector adhesion preventive member have an overlap of not less than 0.1 mm and not more than 200 mm in a flow direction of gas between the gas-introducing opening section and the exhaust opening section, and
the film forming chamber adhesion preventive member and the exhaust adhesion preventive member have an overlap of not less than 0.1 mm and not more than 200 mm in a flow direction of gas between the gas-introducing opening section and the exhaust opening section.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the injector adhesion preventive member is configured such that its sideward outer surface is located inside at a distance of not less than 0.1 mm and not more than 200 mm with reference to a side end of the plate electrode, and
the exhaust adhesion preventive member is configured such that its sideward outer surface is located inside at a distance of not less than 0.1 mm and not more than 200 mm with reference to a side end of the plate electrode end.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the film forming chamber adhesion preventive member, the injector adhesion preventive member, and the exhaust adhesion preventive member are mounted and fixed to the film forming chamber so as to each have a fixing end section against the film forming chamber at a position of a distance of not less than 50 mm apart from a proximal plate electrode end.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the film forming chamber adhesion preventive member has a length extending over the injector adhesion preventive member and the exhaust adhesion preventive member.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the upper inert-gas supply section and the lower inert-gas supply section are respectively connected to the upper inert-gas supply port and the lower inert-gas supply port by a shower head structure.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
each of an upper surface of the injector adhesion preventive member and an upper surface of the exhaust adhesion preventive member is separated from a lower surface of the plate electrode side by a gap of not less than 0.1 mm and not more than 20 mm in vertical distance.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
each of the injector adhesion preventive member and the exhaust adhesion preventive member is separated from a proximal end section of the substrate retained by the counter electrode by a gap of not less than 0.1 mm and not more than 200 mm in horizontal distance, in a flow direction of gas between the gas introducing section and the exhaust section.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
each of a lower surface of the injector adhesion preventive member and a lower surface of the exhaust adhesion preventive member is separated from an upper surface of the counter electrode side by a gap of not less than 0.1 mm and not more than 20 mm in vertical distance.
Invention of the apparatus for plasma atomic layer deposition of another embodiment is the present invention of the above described embodiment, in which
the counter electrode includes a counter electrode retaining section which has a retaining surface for retaining the substrate, and a counter-electrode peripheral edge section which is present around the counter electrode retaining section, and has a height lower than that of the counter electrode retaining surface.
According to the present invention, the area of film adhesion within the film forming chamber can be reduced, thereby making it possible to suppress generation of particles and to reduce the frequency of cleaning the film forming chamber and the adhesion preventive member.
First, referring to the appended drawings, the configuration of an apparatus for plasma atomic layer deposition 10 of the present embodiment will be described.
The apparatus for plasma atomic layer deposition 10 of the present embodiment alternately supplies a raw material gas and a reaction gas to form a thin film in units of atomic layers on a substrate 100. In that occasion, to improve the reaction activity, the substrate 100 can be heated. In the present embodiment, TMA (Tri-Methyl Aluminum) is used as the raw material gas, and in that occasion, plasma is generated to improve reaction activity. In the present embodiment, a parallel plate electrode is used to generate plasma.
The film forming chamber 11 includes an injector 21, an exhaust flange 31, a plate electrode 12, a counter electrode 14, and a high-frequency power supply 16. The counter electrode 14 includes a stage heater 14A, and can adjust the temperature of the substrate 100. For example, in the case of the apparatus for plasma atomic layer deposition, the substrate 100 is heated to 50 to 200° C. When carrying out the processing, the film forming chamber 11 is maintained in vacuum.
The plate electrode 12 is provided above the substrate 100 separated by a film forming space S, and is supported by an insulating support 41. A surface exposed from the insulating support 41 functions as the plate electrode 12, and an end of the exposed surface corresponds to the end section of the plate electrode 12. A conductive, plate-shaped plate electrode adhesion preventive member 13 is provided on the side of the lower surface where the plate electrode 12 is exposed, and the lower surface of the plate electrode adhesion preventive member 13 and the lower surface of the insulating support 41 are made flush with each other.
Moreover, the counter electrode 14 includes, around a counter-electrode retaining section 14B having a retaining surface for retaining the substrate 100, a counter-electrode peripheral edge section 14C whose height is made smaller than that of the retaining surface, and is retained to the film forming chamber 11 by a stage stopper 17 at the counter-electrode peripheral edge section 14C. Further, a plate-shaped counter electrode adhesion preventive member 15 is provided on an upper surface of the counter-electrode peripheral edge section 14C and a vertical surface of the border with the retaining surface.
By the high-frequency power supply 16 supplying high-frequency current of a predetermined frequency to the plate electrode 12, plasma is generated between the plate electrode 12 and the counter electrode 14.
Next, the gas introducing section 20 through which a raw material gas, a reaction gas, and a purge gas are introduced will be described. The gas introducing section 20 supplies the raw material gas, reaction gas, and purge gas into the film forming chamber 11 according to a processing procedure. The injector 21 is mounted to the gas-introducing opening section 11A of the film forming chamber 11, and the injector adhesion preventive member 22 is inserted into the gas-introducing opening section 11A from inside the film forming chamber 11 and mounted thereto so as to surround the opening of the gas-introducing opening section 11A. The injector adhesion preventive member may have any configuration such as to surround the opening by being inserted thereto, surround it from outside, or combination thereof.
Note that, in this example, the gas-introducing opening section 11A is formed into a rectangular-hole shape, and the injector adhesion preventive member 22 is disposed in a rectangular-tube shape so as to surround the gas-introducing opening section 11A. The injector adhesion preventive member 22 may be one which is formed into a tubular shape, or one which is made into a tubular shape by joining multiple members. The injector adhesion preventive member may be any of configurations including one to surround the opening by being inserted into the opening section, one to surround the opening from outside, or combination thereof.
Next, an exhaust section 30 will be described. The exhaust section 30 exhausts the raw material gas, reaction gas, and purge gas from the film forming chamber 11 according to the processing procedure. The exhaust flange 31 is mounted to an exhaust opening section 11B of the film forming chamber 11, and an exhaust adhesion preventive member 32 is inserted into the exhaust opening section 11B from inside the film forming chamber 11, and mounted thereto so as to surround the opening of the exhaust opening section 11B. The exhaust adhesion preventive member may have any configuration including one to be inserted into the opening section to surround the opening, one to surround the opening from outside, and the combination thereof.
Note that, in this example, the exhaust opening section 11B is formed into a rectangular-hole shape, and the exhaust adhesion preventive member 32 is disposed in a rectangular-tube shape so as to surround the exhaust opening section 11B. The exhaust adhesion preventive member 32 may be formed into a tubular shape, or made tubular by joining multiple members. The exhaust adhesion preventive member 32 may be made into a tubular shape conforming to the shape of the exhaust opening section 11B.
The gas introduced into the film forming chamber 11 results in a flow of gas from the gas introducing section 20 toward the exhaust section 30 according to the processing procedure. The following description will be given with supposition that the direction intersecting with this flow of gas be a sideward direction.
The injector adhesion preventive member 22 which is an insulator is mounted by being inserted from inside the film forming chamber 11 and is fixed to the film forming chamber 11 with a fixing screw 23.
An injector adhesion preventive member upper plate 22A corresponding to the upper side of the injector adhesion preventive member 22 is separated from the plate electrode adhesion preventive member 13 provided on the plate electrode 12 side by a gap in the vertical direction, and an injector adhesion preventive member lower plate 22B corresponding to the lower side of the injector adhesion preventive member 22 is separated from the counter electrode adhesion preventive member 15 on the counter electrode 14 side by a gap in the vertical direction.
Moreover, a film forming chamber adhesion preventive member 63 is disposed on each side of the injector adhesion preventive member 22 and the exhaust adhesion preventive member 32 to be mounted and fixed to an inner wall of the film forming chamber 11. In this example, it is placed on a projecting wall 64 which projects from the inner wall of the film forming chamber 11, and is fixed to the projecting wall 64 with a fixing screw 65. A film forming chamber adhesion preventive member 63 has an enough size to cover a vertical width of an injector adhesion preventive member side plate 22C of the injector adhesion preventive member 22, and further has a length extending over the injector adhesion preventive member side plate 22C and an exhaust adhesion preventive member side plate 32C.
An inner surface of the film forming chamber adhesion preventive member 63 is separated from an outer surface of the injector adhesion preventive member side plate 22C and an outer surface of the exhaust adhesion preventive member side plate 32C by gaps, and further the film forming chamber adhesion preventive member 63 is separated from the insulating support 41, the plate electrode adhesion preventive member 13, the counter electrode adhesion preventive member 15, and the substrate 100 retained by the counter electrode 14 by gaps.
The space inside the injector adhesion preventive member 22, the exhaust adhesion preventive member 32, and the film forming chamber adhesion preventive member 63 constitutes a film forming space S.
The film forming chamber 11 is connected with an upper inert-gas supply section 51 and a lower inert-gas supply section 52, in which the upper inert-gas supply section 51 is connected to an upper inert-gas supply port 53 provided inside the film forming chamber 11, and the lower inert-gas supply section 52 is connected to a lower inert-gas supply port 54 provided inside the film forming chamber 11. The upper inert-gas supply section 51 and the lower inert-gas supply section 52 can supply inert gas such as nitrogen.
The inert gas ejected from the upper inert-gas supply port 53 is supplied into the film forming chamber 11 through gaps formed by the injector adhesion preventive member upper plate 22A, and the insulating support 41, the plate electrode 12, and the plate electrode adhesion preventive member 13.
Moreover, the inert gas ejected from the upper inert-gas supply port 53 is supplied into the film forming chamber 11 through gaps formed by the exhaust adhesion preventive member upper plate 32A, and the insulating support 41, the plate electrode 12, and the plate electrode adhesion preventive member 13.
Further, the inert gas ejected from the upper inert-gas supply port 53 is supplied to the film forming chamber 11 through gaps formed by the film forming chamber adhesion preventive member 63, and the insulating support 41, the plate electrode 12, and the plate electrode adhesion preventive member 13.
The inert gas ejected from the lower inert-gas supply port 54 is supplied into the film forming chamber 11 through gaps formed by the injector adhesion preventive member lower plate 22B, and the counter electrode 14, the counter electrode adhesion preventive member 15, and the substrate 100 retained by the counter electrode 14.
Moreover, the inert gas ejected from the lower inert-gas supply port 54 is supplied into the film forming chamber 11 through gaps formed by the exhaust adhesion preventive member lower plate 32B, and the counter electrode 14, the counter electrode adhesion preventive member 15, and the substrate 100 retained by the counter electrode 14.
Further, inert gas ejected from the lower inert-gas supply port 54 is supplied to the film forming chamber 11 through gaps formed by the film forming chamber adhesion preventive member 63, and the counter electrode 14, the counter electrode adhesion preventive member 15, and the substrate 100 retained by the counter electrode 14.
Here, the injector adhesion preventive member 22 is preferably configured such that a tip end of the injector adhesion preventive member upper plate 22A is located inside from an end section of the plate electrode 12, and further, extends over a horizontal distance “a” of not less than 0.1 mm and not more than 200 mm in a direction toward the plate electrode center with reference to the end section of the plate electrode 12. A larger value of the horizontal distance “a” makes it possible to suppress the raw material gas and reaction gas from infiltrating to the upper inert-gas supply port 53 side from an outlet of the injector adhesion preventive member 22. However, since a larger value of the horizontal distance “a” causes increase in the size of the film forming chamber 11, an optimum value is needed. In the apparatus for plasma atomic layer deposition of the present invention, an upper limit thereof is preferably 20 mm.
Moreover, as shown in
A smaller value of the vertical distance “b” makes it possible to suppress the raw material gas and reaction gas from infiltrating to the upper inert-gas supply port 53 side. However, an extremely small value of the vertical distance “b” may cause interference between the injector adhesion preventive member 22 and the insulating support 41 depending on machining accuracy of the film forming chamber 11, possibly leading to breakage. Since a larger value of the vertical distance “b” allows the raw material gas and reaction gas to infiltrate to the upper inert-gas supply port 53 side from the injector adhesion preventive member 22 outlet, an optimum value will be needed. In the apparatus for atomic layer deposition of the present invention, an upper limit thereof is preferably 3 mm.
Moreover, the injector adhesion preventive member 22 needs to be an insulator. Because, when it is a metal, electric discharge occurs between the plate electrode 12 and the injector adhesion preventive member 22. For example, by making the injector adhesion preventive member 22 with alumina ceramic, it is possible to suppress electric discharge.
Moreover, the injector adhesion preventive member 22 is, as shown in
Moreover, as shown in
Moreover, the injector adhesion preventive member 22 is, as shown in
Exactly the same as regarding the gas introducing section 20 applies to the exhaust section 30. It is preferable that the gas introducing section 20 and the exhaust section 30 are symmetrical. Therefore, it is desirable that the exhaust adhesion preventive member 32 also satisfies the above described conditions in the distances “a” to “e”. In this case, the same conditions are presented with the injector adhesion preventive member 22 being replaced with the exhaust adhesion preventive member 32.
In the relation between a sideward end of the plate electrode 12 and an inner side surface of the film forming chamber adhesion preventive member 63, it is desirable that the inner side surface of the film forming chamber adhesion preventive member 63 is located inwardly to the sideward end of the plate electrode 12, and the horizontal distance “j” in that case is preferably not less than 0.1 mm and not more than 200 mm. A larger value of “j” makes it possible to suppress the raw material gas and the reaction gas from infiltrating to the film forming chamber adhesion preventive member 63 side. However, a larger value leads to a larger size of the film forming chamber, an optimum value is needed. In the present apparatus for atomic layer deposition, it is preferably 20 mm.
Moreover, fixing of the film forming chamber adhesion preventive member 63 is preferably performed at a point having a horizontal distance “g” of not less than 50 mm from an end surface of the plate electrode 12 as shown in
Further,
Moreover, an overlapping distance “i” in the flow direction of gas between the injector adhesion preventive member 22 and the film forming chamber adhesion preventive member 63 is preferably not less than 0.1 mm and not more than 200 mm, and further the distance from the overlapping section to the fixing screw 23 is preferably 120 mm. A larger value of the distance “i” makes it possible to suppress the raw material gas and the reaction gas from infiltrating to the film forming chamber 11 inner wall side.
Exactly the same as regarding the injector adhesion preventive member 22 applies to the exhaust adhesion preventive member 33 as well. Therefore, it is desirable that distances “f” to “j” satisfy each of the above described conditions, in the exhaust adhesion preventive member 33 as well. In this case, the same conditions are presented with the injector adhesion preventive member 22 being replaced with the exhaust adhesion preventive member 32.
Moreover, the lower inert-gas supply section 52 may have a similar structure to that of the upper inert-gas supply section 51, and further may have a structure in which one supply section is provided, and then branched to the upper inert-gas supply ports and the lower inert-gas supply section ports. A shower-hole diameter at each supply port is preferably within a range of 1 to 3 mm, and may be about 1 mm. A shower-hole pitch is preferably 10 mm to 200 mm. The shower may be made by providing through holes in the film forming chamber 11, or a shower plate is separately made and may be mounted to the film forming chamber 11.
Next, the processing procedure in the apparatus for plasma atomic layer deposition 10 will be described.
First, the raw material gas supply section supplies a raw material gas into the film forming chamber 11 (step s1). Specifically, it supplies the raw material gas to the gas introducing section 20 (step s1). The raw material gas is supplied into the film forming chamber 11. The raw material gas is supplied into the film forming chamber 11 for 0.1 seconds, for example. As shown in
Moreover, in step s1, inert gas is supplied to an inner surface of the injector 21 and an outer surface of the injector adhesion preventive member 22. Further, in the exhaust section 30, inert gas is also supplied to the exhaust flange 31 and the exhaust adhesion preventive member 32. Furthermore, inert gas is supplied into the film forming chamber also from the upper inert-gas supply section 51 and the lower inert-gas supply section 52.
In the present embodiment, by supplying inert gas not only in step s1, but constantly including in steps s2 to s4 when the raw material gas is supplied, it is possible to suppress the raw material gas from penetrating into:
a gap between the film forming chamber 11 and the injector 20,
a gap between the film forming chamber 11 and the injector adhesion preventive member 22,
a gap between the injector adhesion preventive member 22 and the insulating support 41,
a gap between the injector adhesion preventive member 22 and the counter electrode adhesion preventive member 15,
a gap between the film forming chamber 11 and the exhaust flange 31,
a gap between the film forming chamber 11 and the exhaust adhesion preventive member 32,
a gap between the exhaust adhesion preventive member 32 and the insulating support 41,
a gap between the exhaust adhesion preventive member 32 and the counter electrode adhesion preventive member 15,
a gap between the film forming chamber adhesion preventive member and the insulating support 41, and
a gap between the film forming chamber adhesion preventive member and the counter electrode adhesion preventive member 15.
Next, supply of the raw material gas is stopped, and a purge gas is supplied at the gas introducing section (step s2). The purge gas is supplied into the film forming chamber 11. The raw material gas is discharged to the outside of the film forming chamber 11 from the exhaust section 30.
The purge gas is supplied into the film forming chamber 11 for, for example, 0.1 second. The exhaust section 30 exhausts a raw material gas 110 and a purge gas 112 within the film forming chamber 11. The exhaust section 30 exhausts the raw material gas 110 and the purge gas 112 within the film forming chamber 11 for, for example, 2 seconds. As shown in
Next, a reaction gas is supplied into the film forming chamber (step s3). Specifically, the reaction gas is supplied through the gas introducing section 20 (step s3). The reaction gas is supplied into the film forming chamber 11 through a passage of the gas introducing section 20. The reaction gas is supplied into the film forming chamber 11 for, for example, 1 second. As shown in
Further, in step s3 as well, inert gas is supplied at the inner surface of the injector 21, the outer surface of the injector adhesion preventive member 22, and the exhaust section 30. Therefore, in step s3, by supplying inert gas when the reaction gas is supplied into the film forming chamber 11, it is possible to suppress the reaction gas from penetrating into:
a gap between the film forming chamber 11 and the injector 20,
a gap between the film forming chamber 11 and the injector adhesion preventive member 22,
a gap between the injector adhesion preventive member 22 and the insulating support 41,
a gap between the injector adhesion preventive member 22 and the counter electrode adhesion preventive member 15,
a gap between the film forming chamber 11 and the exhaust flange 31,
a gap between the film forming chamber 11 and the exhaust adhesion preventive member 32,
a gap between the exhaust adhesion preventive member 32 and the insulating support 41,
a gap between the exhaust adhesion preventive member 32 and the counter electrode adhesion preventive member 15,
a gap between the film forming chamber adhesion preventive member and the insulating support 41, and
a gap between the film forming chamber adhesion preventive member and the counter electrode adhesion preventive member 15.
Next, the supply of the reaction gas is stopped, and a purge gas is supplied at the gas introducing section (step s4). The purge gas is supplied into the film forming chamber 11. The purge gas is discharged from the exhaust section 30 to the outside of the film forming chamber 11. The purge gas is supplied into the film forming chamber 11 for, for example, 0.1 second. The exhaust section 30 exhausts the reaction gas 114 and the purge gas 112 within the film forming chamber 11. As shown in
Through steps s1 to s4 described so far, a thin-film layer 104 of one atomic layer is formed on the substrate 100. Hereinafter, by repeating steps s1 to s4 for predetermined times, it is possible to form a thin-film layer 104 having a desired film thickness.
Since, in the apparatus for plasma atomic layer deposition 10 of the present embodiment, the inert-gas flows on the inner surface of the injector 21 and the outer surface of the injector adhesion preventive member 22, it is possible to suppress the raw material gas and the reaction gas from penetrating into the gap between the film forming chamber 11 and the injector 21. For that reason, it is possible to suppress a thin film from adhering in a gap between the film forming chamber 11 and the injector 21. Moreover, the exhaust section 30 is also prevented from adhesion of thin film in a similar fashion.
Further, inert gas is also supplied from the upper inert-gas supply section 51 and the lower inert-gas supply section 52, making it possible to suppress film adhesion within the film forming chamber.
Moreover, for example, an alumina film, which is formed by using TMA as the raw material gas, and O3 as the reaction gas, can be subjected to gas etching by BCl3 gas. To subject an alumina film to gas etching with BCl3 gas, for example, it needs to be heated to a high temperature of about 500° C.
The inner wall of the film forming chamber 11 located in the vicinity of a stage heater 14A can be heated by the stage heater 14A to a high temperature of about 500° C. For that reason, a thin film which has adhered to the inner wall of the film forming chamber 11 located in the vicinity of the stage heater 14A can be removed by gas etching.
As so far described, since, according to the present embodiment, it is possible to suppress a thin film from adhering to the inner wall of the film forming chamber 11 and to remove the film which has adhered to the inner wall by gas etching, it is possible to reduce the frequency of cleaning by wet etching.
By using the apparatus for plasma atomic layer deposition shown in the embodiment, an AlON thin film was formed on G2 glass substrate of 370 mm×470 mm. Various values of the present apparatus for atomic layer deposition were as follows:
a: 20 mm,
b: 3 mm,
c: 100 mm,
d: 3 mm,
e: 100 mm,
f: 100 mm,
g: 100 mm,
h: 1 mm,
i: 120 mm,
j: 20 mm,
Shower-hole diameter: 1 mm, and
Shower pitch: 100 mm.
TMA (trimethyl aluminum) was used as the liquid raw material (Al source), and Oxygen plasma and nitrogen plasma were used as the reaction gas. Film forming was carried out according to the sequence shown in
After film forming of 20 μm was performed, portions where film adhesion was observed within the film forming space were only the injector, the injector adhesion preventive member, the exhaust adhesion preventive member, the plate electrode adhesion preventive member, two film forming chamber adhesion preventive members, and the counter electrode adhesion preventive member; and generation of powder was not observed. Objects to be maintained included only the above described 6 items of adhesion preventive member, and 20 pieces of screws used in the upper electrode adhesion preventive member, and thus maintenability was remarkably improved.
Although the present invention has been described based on the above described embodiment and Example so far, appropriate modifications may be made to the above described contents as long as they do not depart from the scope of the present invention.
The present application claims priority to Japanese Patent Application No. 2015-106858, filed on May 26, 2015 in Japan, the entirety of which is incorporated herein by reference.
Number | Date | Country | Kind |
---|---|---|---|
2015-106858 | May 2015 | JP | national |
Filing Document | Filing Date | Country | Kind |
---|---|---|---|
PCT/JP2016/062402 | 4/19/2016 | WO | 00 |
Publishing Document | Publishing Date | Country | Kind |
---|---|---|---|
WO2016/190007 | 12/1/2016 | WO | A |
Number | Name | Date | Kind |
---|---|---|---|
4793283 | Sarkozy | Dec 1988 | A |
5044314 | McNeilly | Sep 1991 | A |
5326725 | Sherstinsky et al. | Jul 1994 | A |
5772770 | Suda | Jun 1998 | A |
5788799 | Steger | Aug 1998 | A |
5972116 | Takagi | Oct 1999 | A |
5997651 | Matsuse et al. | Dec 1999 | A |
6194037 | Terasaki | Feb 2001 | B1 |
6248672 | Takagi | Jun 2001 | B1 |
6527911 | Yen | Mar 2003 | B1 |
6733593 | Tanaka et al. | May 2004 | B1 |
8430960 | Sumakeris | Apr 2013 | B2 |
9777371 | Coutu | Oct 2017 | B2 |
20020122885 | Ahn | Sep 2002 | A1 |
20020182876 | Kawai | Dec 2002 | A1 |
20030150560 | Kinnard | Aug 2003 | A1 |
20030207032 | Ahn | Nov 2003 | A1 |
20030213560 | Wang | Nov 2003 | A1 |
20060185590 | Schaepkens | Aug 2006 | A1 |
20060280868 | Kato et al. | Dec 2006 | A1 |
20070051312 | Sneh | Mar 2007 | A1 |
20080261074 | Shishikura | Oct 2008 | A1 |
20090277389 | Kakimoto | Nov 2009 | A1 |
20100047447 | Cook | Feb 2010 | A1 |
20100210092 | You | Aug 2010 | A1 |
20100298738 | Felts | Nov 2010 | A1 |
20110174441 | Yamashita | Jul 2011 | A1 |
20110303147 | Tachibana et al. | Dec 2011 | A1 |
20110305836 | Murata et al. | Dec 2011 | A1 |
20120031748 | Ishihara | Feb 2012 | A1 |
20120064245 | Coutu | Mar 2012 | A1 |
20140008352 | Uemura | Jan 2014 | A1 |
20160148801 | Yabe | May 2016 | A1 |
20180315626 | Franklin | Nov 2018 | A1 |
Number | Date | Country |
---|---|---|
101356630 | Jan 2009 | CN |
61163279 | Jul 1986 | JP |
63076880 | Apr 1988 | JP |
01183113 | Jul 1989 | JP |
06140379 | May 1994 | JP |
07201754 | Aug 1995 | JP |
08186081 | Jul 1996 | JP |
09115993 | May 1997 | JP |
11335849 | Dec 1999 | JP |
2000208439 | Jul 2000 | JP |
2000243711 | Sep 2000 | JP |
2002302770 | Oct 2002 | JP |
2003068657 | Mar 2003 | JP |
2004339581 | Dec 2004 | JP |
2006080148 | Mar 2006 | JP |
2006351655 | Dec 2006 | JP |
2007281150 | Oct 2007 | JP |
2009062579 | Mar 2009 | JP |
2010212433 | Sep 2010 | JP |
2010212434 | Sep 2010 | JP |
2010212434 | Sep 2010 | JP |
2012052221 | Mar 2012 | JP |
2012126977 | Jul 2012 | JP |
2012175055 | Sep 2012 | JP |
2014192379 | Oct 2014 | JP |
2015073019 | Apr 2015 | JP |
2015073020 | Apr 2015 | JP |
2015073021 | Apr 2015 | JP |
1020080098687 | Nov 2008 | KR |
101028605 | Apr 2011 | KR |
457524 | Oct 2001 | TW |
0042235 | Jul 2000 | WO |
2007116940 | Oct 2007 | WO |
Entry |
---|
English translation of the International Preliminary Report on Patentability dated Dec. 7, 2017 issued in counterpart International Application No. PCT/JP2016/062402. |
Related U.S. Appl. No. 15/575,357; First Named Inventor: Tatsuya Matsumoto; Title: “Device for Atomic Layer Deposition”; filed: Nov. 18, 2017. |
Related U.S. Appl. No. 15/575,358; First Named Inventor: Tatsuya Matsumoto; Title: “Device for Atomic Layer Deposition”; filed: Nov. 18, 2017. |
Related U.S. Appl. No. 15/575,359; First Named Inventor: Tatsuya Matsumoto; Title: “Atomic Layer Growth Device and Atomic Layer Growth Device Exhaust Unit”; filed: Nov. 18, 2017. |
International Search Report (ISR) and Written Opinion dated Aug. 2, 2016 issued in International Application No. PCT/JP2016/062402. |
Number | Date | Country | |
---|---|---|---|
20180148842 A1 | May 2018 | US |