1. Field of Art
The present invention relates to depositing one or more layers of materials on a substrate using atomic layer deposition (ALD).
2. Description of the Related Art
An atomic layer deposition (ALD) is a thin film deposition technique for depositing one or more layers of material on a substrate. ALD uses two types of chemical, one is a source precursor and the other is a reactant precursor. Generally, ALD includes four stages: (i) injection of a source precursor, (ii) removal of a physical adsorption layer of the source precursor, (iii) injection of a reactant precursor, and (iv) removal of a physical adsorption layer of the reactant precursor. ALD can be a slow process that can take an extended amount of time or many repetitions before a layer of desired thickness can be obtained. Hence, to expedite the process, a vapor deposition reactor with a unit module (so-called a linear injector), as described in U.S. Patent Application Publication No. 2009/0165715 or other similar devices may be used to expedite ALD process. The unit module includes an injection unit and an exhaust unit for a source material (a source module), and an injection unit and an exhaust unit for a reactant (a reactant module).
A conventional ALD vapor deposition chamber has one or more sets of reactors for depositing ALD layers on substrates. As the substrate passes below the reactors, the substrate is exposed to the source precursor, a purge gas and the reactant precursor. The source precursor molecules deposited on the substrate reacts with reactant precursor molecules or the source precursor molecules are replaced with the reactant precursor molecules to deposit a layer of material on the substrate. After exposing the substrate to the source precursor or the reactant precursor, the substrate may be exposed to the purge gas to remove excess source precursor molecules or reactant precursor molecules from the substrate.
To reduce the number of reiteration needed to deposit a material of a desired thickness, it is advantageous to increase the deposition rate per each ALD cycle.
Embodiments relate to depositing a layer of material on a substrate by generating radicals of a gas mixture containing a first gas and a second gas and then injecting the radicals onto a substrate. The first gas includes a nitrogen compound. The substrate is previously injected with a source precursor. The radicals function as a reactant precursor reacting with or replacing source precursor molecules on the substrate and depositing a layer of material on the substrate.
In one embodiment, the second gas includes another nitrogen compound. The first gas may include NH3 and the second gas may include N2O.
In one embodiment, the deposited material comprises aluminum oxynitride (AlON).
In one embodiment, the ratio of N2O and NH3 is 70:30 to 90:10. More preferably, the ratio of N2O and NH3 is 80:20.
In one embodiment, the mixture of gases is injected into a plasma chamber in a radical reactor. A voltage is applied between a first electrode in the plasma chamber and a second electrode surrounding the plasma chamber to generate plasma in the plasma chamber. The plasma generates radicals of the mixture of gases.
In one embodiment, the distance from the plasma chamber to the substrate is less than 80 mm.
In one embodiment, the source precursor is selected from a group consisting of Tetraethylmethylaminozirconium (TEMAZr), Trimethylsilane (TMS), Tridimethylaminesilicone (3DMAS) and Tetraethylmethylaluminumtitanium (TEMATi).
In one embodiment, the first gas comprises NH3 and the second gas comprises CH4.
Embodiments also relate to a radical reactor comprising a body and an electrode to generate radicals functioning as a reactant precursor in an atomic layer deposition (ALD) process. The body is formed with a channel for supplying gas, a plasma chamber connected to the channel to receive the supplied gas and generate radicals of the supplied gas, a reaction chamber connected to the plasma chamber to receive the generated radicals and located above a substrate to expose the substrate to the radicals, and one or more exhaust portions to discharge excess gas and/or radicals. An electrode extends within the body. A voltage is applied across the electrode and the body to generate plasma in the plasma chamber.
Embodiments are described herein with reference to the accompanying drawings. Principles disclosed herein may, however, be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein. In the description, details of well-known features and techniques may be omitted to avoid unnecessarily obscuring the features of the embodiments.
In the drawings, like reference numerals in the drawings denote like elements. The shape, size and regions, and the like, of the drawing may be exaggerated for clarity.
Embodiments relate to performing atomic layer deposition (ALD) using a gas mixture to generate radicals that function as a reactant precursor for depositing a layer of material on a substrate. The gas mixture includes a nitrogen containing compound such as NH3 or N2O. The substrate is previously injected with a source precursor material. Hence, when the substrate is injected with the reactant precursor, a layer of material is deposited on the substrate. By using a mixture of gases instead of a single gas to generate radicals, the deposition rate of the material can be increased.
The process chamber enclosed by the walls may be maintained in a vacuum state to prevent contaminants from affecting the deposition process. The process chamber 110 contains a susceptor 128 which receives a substrate 120. The susceptor 128 is placed on a support plate 124 for a sliding movement. The support plate 124 may include a temperature controller (e.g., a heater or a cooler) to control the temperature of the substrate 120. The linear deposition device 100 may also include lift pins (not shown) that facilitate loading of the substrate 120 onto the susceptor 128 or dismounting of the substrate 120 from the susceptor 128.
In one embodiment, the susceptor 128 is secured to brackets 210 that move across an extended bar 138 with screws formed thereon. The brackets 210 have corresponding screws formed in their holes receiving the extended bar 138. The extended bar 138 is secured to a spindle of a motor 114, and hence, the extended bar 138 rotates as the spindle of the motor 114 rotates. The rotation of the extended bar 138 causes the brackets 210 (and therefore the susceptor 128) to make a linear movement on the support plate 124. By controlling the speed and rotation direction of the motor 114, the speed and the direction of the linear movement of the susceptor 128 can be controlled. The use of a motor 114 and the extended bar 138 is merely an example of a mechanism for moving the susceptor 128. Various other ways of moving the susceptor 128 (e.g., use of gears and pinion at the bottom, top or side of the susceptor 128). Moreover, instead of moving the susceptor 128, the susceptor 128 may remain stationary and the reactors 136 may be moved.
One or more of the reactors 320A, 320B, 334A, 334B, 364A, 364A, 368B, 368B are connected to gas pipes (not shown) to provide source precursor, reactor precursor, purge gas and/or other materials. The materials provided by the gas pipes may be (i) injected onto the substrate 314 directly by the reactors 320A, 320B, 334A, 334B, 364A, 364B, 368A, 368B, (ii) after mixing in a chamber inside the reactors 320A, 320B, 334A, 334B, 364A, 364B, 368A, 368B, or (iii) after conversion into radicals by plasma generated within the reactors 320A, 320B, 334A, 334B, 364A, 364B, 368A, 368B. After the materials are injected onto the substrate 314, the redundant materials may be exhausted through outlets 330, 338. The interior of the rotating deposition device 300 may also be maintained in a vacuum state.
Although following example embodiments are described primarily with reference to the reactors 136 in the linear deposition device 100, the same principle and operation can be applied to the rotating deposition device 300 or other types of deposition device.
In one or more embodiments, the reactor 136A is a gas injector that injects source precursor materials onto the substrate 120. The reactor 136A is connected to a pipe (not shown) to receive the source precursor from a source (e.g., a canister). The source precursor is injected onto the substrate 120, forming one or more layers of source precursor molecules on the substrate 120. Excess source precursor molecules are exhausted via exhaust pipes 422A, 422B.
The reactor 136B may be a radical reactor that generates radicals of gas or a gas mixture received from one or more sources (e.g., canisters). The radicals of gas or gas mixture may function as reactant precursor that forms an atomic layer of materials on the substrate 120 in conjunction with the source precursor. The gas or gas mixtures are injected into the reactor 136B via a pipe (not shown), and are converted into radicals within the reactor 136B by applying voltage across electrodes. The radicals are injected onto the substrate 120, and remaining radicals and/or gas reverted to inactive state are discharged from the reactor 136B via exhaust pipes 438A, 438B.
While the source precursor molecules pass the constriction zones 518A, 518B, physisorbed source precursor molecules are at least partially removed from the region of the substrate 120 below these zones 518A, 518B due to higher flow rate of the source precursor molecules.
In one or more embodiment, the injector 136A may also inject purge gas onto the substrate 120 to remove physisorbed source precursor molecules from the substrate 120, leaving only chemisorbed source precursor molecules on the substrate 120. In this way, an ALD process yielding a high quality atomic layer can be obtained.
The radical reactor 136B has a similar structure as the injector 136A except that the radical reactor further includes a plasma generator. The plasma generator includes an inner electrode 576 and an outer electrode 572 surrounding a plasma chamber 578 (the outer electrode 572 may be part of a metallic body 550). The body 550 is formed with, among others, a gas channel 564, perforations (slits or holes) 568, the plasma chamber 578, an injector slit 580, a reaction chamber 562 and exhaust portions 560A, 560B. A gas or a mixture of gases is injected via the channel 564 and perforations 568 into the plasma chamber 578. By applying a voltage difference between the inner electrode 576 and the outer electrode 572, plasma is generated in the plasma chamber 578. As a result of the plasma, radicals of the gas or the mixture of gases are generated within the plasma chamber 578. The generated radicals are injected into the reaction chamber 562 via the injector slit 580. The region of the substrate 120 below the reaction chamber 562 comes into contact with the radicals, forming the deposited layer 410 on the substrate 120.
The distance H between the plasma chamber 578 and the substrate 120 is configured so that a sufficient amount of radicals reach the substrate 120 in an active state. Radicals have a predetermined lifetime. Hence, as the radicals travel via the injector slit 580 and the reaction chamber 562 to the substrate 120, some of the radicals revert back to an inactive gaseous state. With the increase in the travel distance, the amount of radicals reverting to the inactive gaseous state increases. Hence, it is advantageous to set the distance H to be less than a certain length. For example, the distance H is set to 10 to 100 mm.
When using radicals of nitrogen containing gas mixtures (e.g., N2O and NH3 mixture), the lifespan of the radicals is relatively short and most of the radicals revert back to an inactive state if the distance H is 80 mm or more. Hence, the distance H is set to be less than 80 mm when using radicals of nitrogen containing gas mixtures.
For the purpose of experiment illustrated in
A gas or mixture of gases is injected into the radical reactor 600 via a channel 618 and perforations 622 formed in the body 610 of the radical reactor. Part 624 of the body 610 functions as an outer electrode. By applying the voltage between the inner electrode 614 and the outer electrode 624, radicals can be generated in a plasma region 628. The radicals flow into the exhaust portions 626A, 626B via constriction zones 642A, 642B. The principle and operation of depositing an atomic layer in the radical reactor 600 are substantially the same as the radical reactor 136B, and are omitted herein for the sake of brevity. Radical reactors of various other configurations may also be used.
When generating radicals of nitrogen, it is advantageous to use a mixture of gases instead of using a single gas. For example, based on experiments, radicals generated from a mixture of N2O gas and NH3 gas resulted in a higher deposition rate compared to using only N2O gas or NH3 gas. However, particles were formed at certain mixture ratio of gases. Hence, experiments were performed to identify a range of mixture ratio that resulted in a higher deposition rate while avoiding the formation of particles in the radical reactor 136B, as described below in detail with reference to Table 1.
In the following experiments, TMA was first injected on the substrate and then injected with radicals of gas(es) to form a film of AlN, Al2O3 or AlON. The temperature of the substrate was maintained at 80° C. and the temperature of TMA gas was maintained at 5° C. To generate radicals used as reactant precursor, NH3, N2O or a mixture thereof was used. To generate the plasma, a voltage signal of 120 kHz at 200 watt was applied between the inner electrode 576 and the outer electrode 572. The distance H (See
The measured deposition rate of AlN, Al2O3 or AlON layer and characteristic of these layers are tabulated in Table 1. When NH3 and N2O were injected into the radical reactor at a ratio of x (for NH3 gas, where x takes a value between 0 and 1) to (1−x)(for N2O gas), the resulting layer was Al2O3 (when x=1), AlN (when x=0) or (x)Al2O3+(1−x)AlN.
As seen in Table 1, the deposition rate was greatest (1.96 Å/cycle) when the ratio between N2O gas and NH3 gas was 80:20. At this ratio, no particle was generated in the radical reactor. When the NH3 was increased or decreased beyond this ratio, the deposition rate decreased. Moreover, as the ratio of NH3 increased to 40%, particles were formed in the radical reactor. Specifically, particles were detected in the radical reactor when ratio of N2O and NH3 ranged from 40:60 to 60:40. The particles were not detected when the ratio of NH3 increased to 70% and above. Table 1 shows that it is advantageous to use the radicals of nitrogen containing gas mixture instead of using only N2O or NH3 to improve the deposition rate.
In another embodiment, Tetraethylmethylaminozirconium (TEMAZr) may be used as the source precursor and similar mixture of (1−x)N2O and (x)NH3 (where x takes a value above 0 and below 0.5) may be used to generate radicals as the reactant precursor to generate a layer of ZrO(1-x)Nx on the substrate.
In still another embodiment, Trimethylsilane (TMS, (CH3)3SiH) or Tridimethylaminesilicone (3DMAS) may be used as the source precursor and a gas of (1−x)NH3 and (x)N2O (where x is above 0 and below 0.5) may be used to generate radicals acting as reactant precursor to obtain a layer of SiOxN(1-x).
The mixture of gas for generating radicals is not limited to nitrogen containing gases. For example, NH3 may be mixed with CH4 to generate N* and C* radicals. In one embodiment, Tetraethylmethylaluminumtitanium (TEMATi) is used as the source precursor and radicals generated from (1−x)NH3 and (x)CH4 (where x is above 0 and below 50) are used as the reactant precursor to form a layer of TiC(1-x)Nx on a substrate.
In still another embodiment, TiCl4 is used as the source precursor and radicals generated from N2 or NH3 gas are used as the reactant precursor to generate an atomic layer of TiN film on a substrate.
In the above embodiments, the distance H from the substrate to the plasma chamber may be set to be less than 80 mm so that most of the radicals may reach the substrate without reverting back to an inactive state.
The radical reactor 136B is injected with a mixture of gas. The gas mixture may include a first gas and a second gas. The first gas may be NH3 and the second gas may be N2O. By using a mixture of two different gases, the deposition rate of the ALD process can be increased. In this example, the deposited layer is AlON.
Although the present invention has been described above with respect to several embodiments, various modifications can be made within the scope of the present invention. Accordingly, the disclosure of the present invention is intended to be illustrative, but not limiting, of the scope of the invention, which is set forth in the following claims.
This application claims priority under 35 U.S.C. §119(e) to co-pending U.S. Provisional Patent Application No. 61/443,556, filed on Feb. 16, 2011, which is incorporated by reference herein in its entirety.
| Number | Date | Country | |
|---|---|---|---|
| 61443556 | Feb 2011 | US |