The present invention relates to semiconductor processing and, more particularly, to an apparatus and method for providing a massively parallel ALD/CVD system.
Chemical Vapor Deposition (CVD) is a widely used deposition process for the growth of thin films on various substrates, including semiconductor wafers. As microelectronics device dimensions are reduced, or scaled down, CVD is an attractive method for the deposition of conformal films over complex device topography. In the field of atomic/molecular level film deposition, a process known as Atomic Layer Deposition (ALD) has emerged as a promising candidate to extend the abilities of CVD techniques. Generally, ALD is a process wherein conventional CVD processes are divided into separate deposition steps that theoretically go to saturation at a single molecular or atomic monolayer thickness and self-terminate. For ALD applications, the molecular precursors are introduced into the reactor separately. Typically, an ALD precursor reaction is followed by inert gas purging of the reactor to remove the precursor from the reactor prior to the introduction of the next precursor.
Commercial ALD systems today include those with a precursor inject flow with respect to the substrate, such as a semiconductor wafer, of “horizontal” or a “vertical” flow design. In the horizontal flow design, the flow is directed across (parallel to) the surface of the wafer. In the vertical inject design, a purge-pump configuration requires that the gas flow actually have both vertical and horizontal components near to and with respect to the wafer plane.
Horizontal flow reactors generally require, as a minimum, the transport of the exposure pulses of the precursor chemical over the diameter of the wafer, whereas vertical flow reactors allow for axi-symmetric injection of the precursor chemical, so that the transport of the exposure pulses is over the radius of the wafer. This means the trailing edge of the precursors for vertical inject is sharper and may be placed closer to the initial edge of sequential reacting precursors, thus minimizing gas phase reactions. These considerations are important in the design of a practical and efficient commercial ALD reactor.
In order to improve throughput of wafers, the semiconductor industry has employed batch processing. However, as wafer diameters increase (e.g. 200 mm and 300 mm wafer diameters or larger), industry preference is for single wafer processing in a reactor chamber. In reference to ALD processes, batch ALD reactors are believed to be difficult to maintain relative to single wafer reactors, which historically have had the capability for in-situ cleans, at least films made by CVD. Films made by single wafer ALD reactors may also be in-situ cleaned if or when appropriate cleaning chemistry(s) are developed. Accordingly, vertical flow designs may be more preferable for practical ALD systems.
The use of single wafer reactors is also more likely to be accepted by the semiconductor industry, since single wafer reactors allow for improved uniformity and high throughput for wafer processing over batch reactors. However, one critical limitation for wider acceptance of ALD is the fact that high throughput processes are difficult to realize with single reactor systems.
It would be advantageous to have a single wafer vertical flow reactor that is also compact and low in profile in its form factor, so that the reactors may be stacked one atop another. Multiple stacked reactors would allow higher throughput per system and improve a given unit area of factory floor space per wafer processed.
Embodiments of the present invention are illustrated by way of example and are not for the purpose of limitation. In the figures of the accompanying drawings, similar references are utilized to indicate similar elements.
A massively parallel ALD/CVD system is described. A plurality of ALD/CVD reactors have a compact, low vertical profile so that the reactors may be vertically stacked. The stacked deposition reactors are coupled to receive a material, such as a semiconductor wafer, from a load lock unit to place in one of the reactors. In one embodiment, separate load lock units corresponding to the reactors are used, so that the wafer may be vertically positioned to the respective height of the vertically stacked reactors when the wafers are to be located in the load lock.
The vertically stacked ALD/CVD reactors have a low height profile, but allow separate gas inlet at the top of a chamber and separate exhaust at the bottom of the chamber to provide a generally axi-symmetric vertical gas flow across the wafer when the wafer is processed in the reactor chambers. The vertical arrangement allows multiple wafers to be processed separately in module housing the multiple reactors.
In one embodiment, the reactor chamber is formed by placing a top plate and a bottom plate onto a frame. The top plate and the bottom may have a particularly shaped recessed regions to form the top and bottom of the chamber conforming to the particular shape. In one embodiment, the top and bottom of the chamber has a cone-shape to improve the generally axi-symmetric gas flow in the chamber. In another embodiment, horn-shaped chamber is used to provide an option to further improve the gas flow. The low profile reactors are individually constructed with a cover plate integrated with and containing a horizontal input conduit and a base plate integrated with and containing a horizontal conduit for exhaust to minimize the total vertical height of the assembled low profile reactors.
In the description below, the present invention is described in reference to various embodiments. The example embodiments are described in terms of depositing film material on a substrate by Atomic Layer Deposition (ALD). Although ALD is described, the method and apparatus may be readily adapted for the practice of Chemical Vapor Deposition (CVD) or variants thereof. However, the practice of the invention is not limited to these processes. Furthermore, the substrate may be of a variety of base materials for depositing subsequent material layers and need not be limited to the deposition of film layers on a semiconductor substrate (wafer). For example, substrates used for manufacture of flat panel displays may readily be the base substrate.
Referring to
The core architecture of the example MPAS 100 shown includes a central vacuum chamber/platform 101, four process modules 102, load locks 103 and associated connections between the various components and assemblies. As will be described below, the process modules includes three low profile Compact ALD Reactors (CARs) 110, so that a total of twelve such CARs (3×4) are present in the example MPAS 100. The actual number of CARs 110 per process module may vary and may be less than or more than three. Similarly, the number of process modules 102 may vary, so that the total number of CARs 110 for a given MPAS 100 may be less than or greater than twelve.
With the noted design of the MPAS 100 having twelve CARs 110, more wafers may be processed in a smaller footprint area when compared to existing ALD equipment tools. Where productivity is defined as a throughput per unit area of factory floor space, MPAS 100 allows for improved productivity due to the compact design of the CARs 110 and the cluster tool environment. Furthermore, the process capability within a processing chamber of an individual vertical flow compact reactor of the CARs 110 may be made compatible with current thermal and plasma assisted ALD (or CVD) processes, thus, permitting the use of a suitable in-situ clean for continuous operation, as well as plasma assisted CVD or ALD. Other economy of scale features apply, such as common chemical source and pump usage for the stacked reactors in a common process module, which reduces the cost to produce, while still allowing the operation of the independent process modules for high availability of the system operation.
For a standard semiconductor wafer processing, such as for a 300 mm wafer implementation, a Front Opening Unified Pod (FOUP) allows for a standard mechanical wafer interface to a factory. The FOUP typically resides opposite a wall 121 (or some other partition) and is placed onto a FOUP support 119. The wall 121 separates two environments, one environment for handling/storing the wafer and the other environment where the MPAS 100 is located. The number of FOUP supports 119 utilized will depend on the particular system and, thus, the actual number of FOUPs present will vary. Three such FOUP supports 119 are shown in
On the other side of the wall 121, a mini-environment interface (referred to as mini-environment 130) is present. The mini-environment 130 is a “clean” entry space (for example, Class 1) between the wafer handling environment and the vertical process module 101. Thus, the FOUPs are linked to the mini-environment 130, so that the loaded wafers are transferred to the mini-environment 130. The mini-environment is used to interface between the atmospheric environment located to the left of the wall 121 (where the FOUPs are located) and the clean environment where the central robotic vacuum chamber 101 and the processing modules 102 are located. Mini-environments of various schemes may be implemented for the mini-environment 130, including mini-environments known in the art.
In the particular embodiment shown, an atmospheric robot 135 is employed in the mini-environment to move the wafers through the mini-environment 130. In one embodiment the robot 135 is specified with a suitable vertical motion (e.g. approximately 24-36 inches) to accommodate the design for efficient transfer of wafers to the load locks and then to the stacked reactors of the processing modules.
Wafers from the FOUP(s) are loaded into the load locks 103 by the atmospheric robot 135 in the mini-environment 130 using appropriate vertical motion. The load locks 103 have vertical positions that at least at one time in the wafer transfer operation nominally match the vertical positions of the vertically stacked CARs 110. Thus, load locks 103 shown are vertically stacked to correspond to the vertically stacked CARs 110. However, common load lock chambers (not vertically stacked) may also be used in other designs, wherein the load lock is provided with a vertical vacuum movement mechanism for the wafers in the load lock, so that wafers may be placed approximately to match the vertical positions of the center-line position of the stacked reactors. The number of load locks 103 to be used may vary from system to system.
A central robot (not shown) is located within the central vacuum chamber 101 and directly above a robot(s) control housing 142. The vacuum robot may or may not be an industry standard component known in the art, however, it may be modified so that it uses multiple end effectors so as to pick and place more than one wafer at a time from the load lock position to transfer wafers to the CARs 110. The central vacuum robot may take one or more wafers at a time from load lock chambers (less than or of the order of 1.5× the diameter of the wafer and a height defined by the number of wafers to be accommodated by the load lock). For example, if there are 24 wafers in each FOUP, and there are 2 load locks, there may be 36 wafers placed in each load lock 103. The load locks are generally placed about the same horizontal plane or level as the center line of the CARs 110. Options for robotic transfer for one or more wafers under one loading motion are possible. For example, 3 wafers may be removed from the load lock 103 and placed into 3 stacked CARs 110 of one process module 102 in one transfer loading motion or operation. This operation may be sequentially repeated for supplying wafers to the other process modules. During the time of transfer of wafers to the CARs 110 of the second (and other) process module(s), ALD deposition process may take place in the previously wafer loaded process module(s).
Thus, the central vacuum chamber 101 includes vacuum robots to transfer wafers from the load locks 103 to the CARs 110. A central vacuum robot control unit 142 may be attached to the bottom of the central vacuum chamber 101 and a second central robot may be attached to the top of the central vacuum robotic chamber 101 for increased flexibility.
It is to be noted that one or more of these robotic units may be designed to have movement in the up-down direction (z-direction). The atmospheric robot 135 in the mini-environment 130 may have z-direction movement, so that the wafers may be loaded to the correct height in the load locks 103, and a control mechanism 140 for vertical motion of wafers within the load lock 103 so as to align at the appropriate height for the corresponding CAR 110. In general, there are options to transport wafers to the CARs by the single motion or combined vertical motion of the atmospheric robot in the mini-environment 130, load lock 103, and/or the central vacuum robot(s) in the central vacuum chamber 101. It is also to be noted that with the embodiments described above, the wafers when transported to or within the location of the load lock(s) 103, may be vertically positioned already for entry into the corresponding CAR 110, so that significant movement beyond that for placement (or hand-off) within the reactor(s) (generally in the order of approximately 1 cm) is not required of the robot(s) in the central vacuum chamber 101.
The central vacuum chamber 101 is positioned as a hub for the four process modules 102 arranged around the periphery. Again the number of such process modules 102 may vary and the exact layout will depend on the particular footprint. However, a typical layout is the arrangement shown in
The process modules 102 houses the CARs 110 in a stacked arrangement and typically disposed so that the CARs 110 are aligned with the horizontal movement of the wafer from the load lock 103. A chemical source 145 is shown located above the process modules 102 to source the various chemicals to the CARs 110. A delivery unit, in form of a gas switching manifold 146 reside between the chemical source 145 and the CARs 110 to control the switching in/out the precursor chemicals being sourced to the CARs 110. Although individual chemical sources 145 are shown for each process module 102 in the example embodiment, other embodiments may employ a common chemical source for delivery of the chemical(s) to all of the process modules 102. If a common chemical source is utilized, the source may be placed in a variety of remote locations. If placed semi-remotely (away from the overhead projection of a process module 102, but still within or nearly within the overhead projection of the cluster platform), the chemicals may be in a common source “box” that contains all the individual chemical sources for the process modules 102.
It is to be noted that a given process module 102 has the chemical source 145, gas switching manifold 146 and the CARs 110 disposed in a vertical arrangement to provide a smaller footprint on the factory floor. Likewise, much of the machinery (e.g. the robotic units and control units) are placed below the load locks 103 and the central vacuum chamber 101, as well as with the module 102. Furthermore, shown in
In the particular embodiment shown, the chemical source 145 is located in the elevated location above the level of the uppermost reactor of a particular process module 102. The elevated chemical source 145 operates as a common chemical source for the corresponding CARs 110 of the same process module 102. The chemical source 145 supplies precursors for the grouped of stacked CARs 110 of the respective process module 102, by using time phased control sequence. One such control sequence is described below in reference to
The CAR unit 200 also includes a cover plate 210 and a base plate 220. The cover plate 210 resides atop the frame 201 to enclose the frame 201 from the top. Likewise, the base plate 220 encloses the frame 201 from the base (bottom). The frame 201 has a cavity region, which when enclosed by the top and base plates 210, 220 operates as a processing chamber 230 for the wafer. Accordingly, when a wafer is inserted through the wafer slot 203 and placed atop the susceptor 207, the wafer is in position in the processing chamber 230 and may be heated by driving electrical power to a resistive heater and allowing the wafer to reach temperature by thermal conductive and/or radiative heat transfer.
As detailed in
The cover plate 210 also includes a recessed region 211, which has a source opening 212 at or proximal to the center of the recessed region 211. A source conduit 213 extends from the opening 212 to a side of the top plate 210, where an inlet port 214 is present. In the particular example, the source conduit 213 extends to the side opposite the exhaust conduit 224. As noted, the source conduit is disposed horizontally and, in the example, integrated with the cover plate 210. Also in the particular example, the conduit 213 leading to the inlet port 214, couples to gas injection lines to introduce precursors and inert gas. Although a single source conduit 213 is shown, multiple conduit lines, openings and/or ports may be used.
The heater assembly piece 205, base plate 220 and cover plate 210 are shown assembled in a particular arrangement in
When assembled, the various components units 201, 202, 205, 207, 210 and 220 form the CAR unit 200. Cross-sections of the assembled CAR unit 200 are detailed in
It is to be noted that a feature of the CARs illustrated in
As noted in
Furthermore, the vertical flow CAR unit 200 has internal reactor configuration designed with a first generally axi-symmetric homelike or cone-like inject surface shape to confine and distribute the reactants and inert purge gases and a second homelike or cone-like surface for obtaining generally axi-symmetric pumping flow for exhaust. The selection of low aspect ratio cylindrically symmetric generally axi-symmetric cone or horn like surfaces are used to help reduce the height and eliminates dead spaces from the comers of the reactor chamber 230. Below the heater assembly, the reverse cone or horn shape surface provides high conductance conduit pathway to the exhaust and limits the desorbtion effects related to back-streaming from dead space to the region above the wafer. The cone or horn like shape have very low aspect rations (height much less than the diameter) to enable the performance of the vertical flow, low profile compact reactor concept. It is to be noted that other surface shapes may also be implemented and the cover and base plate recessed shapes need not be limited to cone or horn like shapes for achieving improved flow.
Referring to
For example, in a stack of three CAR units 200, the upper reactor is pulsed with an A precursor first and the A pulse is completed before the center reactor is A pulsed, and the lower reactor is A pulsed after the center reactor has completed it's A pulse. Each sequentially A exposure draws precursor from a common chemical precursor source for its process module. Subsequently, the sequence of pulses is repeated for the second precursor B. In between the A and B precursor injection pulses, purge gas flows in the chamber to remove the earlier precursor or any byproducts before the new precursor is introduced.
Thus, a novel vertical flow CAR integrated with MPAS is described with gas inlets and outputs vertically configured into and out of the processing chamber. The low profile allows compact stacking to place multiple reactors in parallel, allowing for dense reactor packing and easy maintenance, but with separate gas injection into and outflow from the reaction chamber, which flow is generally axi-symmetric. The reactor has external geometry that is low profile and substantially rectilinear in its envelope surface.
Furthermore, CARs may be rack mounted, one over the other in a process module to make a vertical stack of independent reactors, so that each reactor may be designed to be removed in a horizontal plane, while the other reactors may continue operation. Precursor and inert purge gases are fed horizontally thru elements 214 and 213 and the exhaust pump flows are carried out horizontally through elements 223 and 224 with respect to the exterior of the CAR to facilitate integration. However, the interior reactor gas flows are vertical with respect to the wafer surface. The exterior shape or form factor of the CAR may be square, rectilinear, round or some other shape. Thermal engineering may be utilized to compensate for proximity effects of upper and lower reactors being in a different thermal environment than the interior (such as the center reactor unit of a three-reactor stack), such as to control the wall temperatures and to assure reactor matching.
Stacked reactors in a given process module may be pumped by being connected to a common or shared pump line. Various options including the combination of dedicated connecting pump lines and shared line (such as a shared manifold line 149 shown in
A reactor is fed its reactant and purge gases by its own dedicated manifold line or as an alternative, use a shared manifold line. One embodiment has an arrangement with its last reactant and inert gas switching valves “close” to each reactor for implementation of rapid gas switching and to the extent possible a similar distance from each inlet orifice leading to the CAR reaction space to achieve matched process performance. Also, individual CAR units may have remotely operable vacuum valves at its wafer input side to be opened for wafer transport into or out of the reactor and closed for process operation of the reactor.
Finally, the MPAS may be computer or processor controlled. Individual stacks of CARs may share a common pump manifold with a single mechanical pump. Individual CARs may be isolated from cross talk with an independently controlled isolation valve for pressure control and gas flow. The process pressure control is independently controlled via hardware and software, such that closed loop pressure control may be permissible from 0 to 10 Torr without affecting the process (deposition or in-situ clean) on the other CAR modules. Also, wafer temperature control from 100 degrees C. to 500 degrees C. and plasma deposition from 10 watts to IKW is in-situ plasma clean is independently controlled without significant crosstalk within the stacked or clustered CARs.
Applications In Alternative Low Cost Manufacturing
In the practical MPAS system described above, the work piece may be a large silicon wafer, (such as a 200 mm or 300 mm wafer). In such cases where robotic wafer transport is not rate limiting, throughputs may be doubled or more compared with state-of-the-art high productivity systems and are particularly well designed for certain ALD applications. These applications would be led by barrier films for interconnect applications, which may have to be 50-100 A, but with ALD deposition rates which are not as large as certain dielectrics. TiN, for example using TiCl4 and NH3 has a deposition rate of about only 0.4 A/cycle, providing about 3 wafers/hr/module for the desired thickness. Thus, a 6 module system may produce only about 18 wph/system, whereas the MPAS provides of order 36 wph/system, that is more suitable for interconnect manufacturing. Since interconnect designs may have 7+ levels of metallization and a level may require the use of an ALD barrier layer, the system cost is prohibitive with the lower ALD system throughput. These MPAS implementations are well suited to semiconductor manufacturing of large area, highly complex chips, such as those of 1 to 2 cm2 and containing billion level transistor component counts, and where the film is used many times for the fabrication of each device and wafer.
The cost of a 300 mm starting wafer is more than nominal and unlikely to be reduced using current silicon crystal pull, cut and polish manufacturing methods. The cost of the wafer itself has been rationalized for silicon semiconductor use against the high value of large area chips using large wafer.
However, some applications may benefit from the use of small wafers, which may cost much less. For example, a 100 mm (4 inch) silicon or compound semiconductor substrate. If a device, such as a system on a chip or a any small commodity part or component may have a cost to produce of only a few dollars, then the MPAS might be used without a FOUP arrangement or even individual 100 mm wafers. One may use a collection of low cost 100 mm substrates or other small work pieces, such as individual or grouped sets of small parts, components or devices carried on a large area (˜300 mm diameter in size) carrier. If 9 such 100 mm wafers were placed on a nominal 300+mm square carrier, then the productivity is 36×9 or 324 w/hr/ MPAS system. This method utilizing large area parallel carrier methods using MPAS and a large number of small form-factor work pieces may be generalized to multiple application.
Thus, massively parallel ALD/CVD deposition system is described.
The present application is a Divisional of U.S. patent application Ser. No. 10/282,609, filed Oct. 29, 2002, entitled “Massively Parallel Atomic Layer Deposition/Chemical Vapor Deposition System”, which claims priority to U.S. Provisional Application No. 60/346,005, filed on Oct. 29, 2001. This patent application is hereby incorporated by reference in its entirety.
Number | Date | Country | |
---|---|---|---|
60346005 | Oct 2001 | US |
Number | Date | Country | |
---|---|---|---|
Parent | 10282609 | Oct 2002 | US |
Child | 11115053 | Apr 2005 | US |