The present invention relates to a plasma enhanced atomic layer deposition system and a method of operating thereof, and more particularly to a method of forming a TaC or TaCN film having good adhesion to Cu.
Typically, during materials processing, plasma is employed to facilitate the addition and removal of material films when fabricating composite material structures. For example, in semiconductor processing, a (dry) plasma etch process is utilized to remove or etch material along fine trenches or within vias or contacts patterned on a silicon substrate. Alternatively, for example, a vapor deposition process is utilized to deposit material along fine lines or within vias or contacts on a silicon substrate. In the latter, vapor deposition processes include chemical vapor deposition (CVD), and plasma enhanced chemical vapor deposition (PECVD).
In PECVD, plasma is utilized to alter or enhance the film deposition mechanism. For instance, plasma excitation generally allows film-forming reactions to proceed at temperatures that are significantly lower than those typically required to produce a similar film by thermally excited CVD. In addition, plasma excitation may activate film-forming chemical reactions that are not energetically or kinetically favored in thermal CVD. The chemical and physical properties of PECVD films may thus be varied over a relatively wide range by adjusting process parameters.
More recently, atomic layer deposition (ALD), a form of CVD or more generally film deposition, has emerged as a candidate for ultra-thin gate film formation in front end-of-line (FEOL) operations, as well as ultra-thin barrier layer and seed layer formation for metallization in back end-of-line (BEOL) operations. In ALD, two or more process gases are introduced alternately and sequentially in order to form a material film one monolayer (or less) at a time. Such an ALD process has proven to provide improved uniformity and control in layer thickness, as well as conformality to features on which the layer is deposited. However, current ALD processes often suffer from contamination problems that affect the quality of the deposited ALD films, and the interfaces between the ALD films and other films in a manufactured device.
The introduction of copper (Cu) metal into multilayer metallization schemes for manufacturing integrated circuits can necessitate the use of diffusion barriers/liners to promote adhesion and growth of the Cu layers and to prevent diffusion of Cu into the dielectric materials. Barriers/liners that are deposited onto dielectric materials can include refractive materials, such as tungsten (W), molybdenum (Mo), and tantalum (Ta), that are non-reactive and immiscible in Cu, and can offer low electrical resistivity. For example, Cu integration schemes for technology nodes less than or equal to 130 nm can utilize a low dielectric constant (low-k) inter-level dielectric, followed by a physical vapor deposition (PVD) of a Ta film or a TaN/Ta film, followed by a PVD Cu seed layer, and an electro-chemical deposition (ECD) Cu fill. Generally, Ta films are chosen for their adhesion properties (i.e., their ability to adhere on low-k films), and TaN/Ta films are generally chosen for their barrier properties (i.e., their ability to prevent Cu diffusion into the low-k film).
The presence of impurities in Ta-containing films can result in weak adhesion between a bulk Cu layer and the Ta-containing films, which in turn can result in electro-migration (EM) and stress migration (SM) problems, as well as reduced device production yields. Thus, new processing methods are needed for improving the properties and integration of Ta-containing films into Cu metallization schemes.
Accordingly, one object of the present invention is directed to improving the properties and integration of Ta-containing films with Cu layers in Cu metallization.
Another object of the present invention is to deposit a TaC or a TaCN film by plasma enhanced atomic layer deposition (PEALD) that has good adhesion to Cu layers.
According to one embodiment of the invention, a method is provided for processing a substrate, the method including disposing the substrate in a process chamber of a PEALD system configured to perform a PEALD process, and depositing a TaC or TaCN film on the substrate using the PEALD process. The PEALD process includes (a) exposing the substrate to a first process material containing tantalum, (b) exposing the substrate to a second process material containing a plasma excited reducing agent, (c) repeating steps (a) and (b) a predetermined number of times, (d) exposing the substrate to plasma excited Argon, and (e) repeating steps (c) and (d) until the TaC or TaCN film has a desired thickness.
According to another embodiment of the invention, a method is provided for processing a substrate, the method including disposing the substrate in a process chamber of a PEALD system configured to perform a PEALD process, and depositing a TaCN film on the substrate using the PEALD process. The PEALD process includes (a) exposing the substrate to a first process material comprising TAIMATA (tertiary amyl imido-tris-dimethylamido tantalum, Ta(NC(CH3)2C2H5)(N(CH3)2)3) in the absence of a plasma, (b) purging the PEALD chamber of the first process material, (c) exposing the substrate to a second process material comprising plasma excited H2, (d) purging the process chamber of the second process material, (e) repeating steps (a)-(d) a desired number of times, (f) exposing the substrate to plasma excited Argon, and (g) repeating steps (a)-(J) until the TaCN film has a desired thickness.
In the accompanying drawings:
In the following description, in order to facilitate a thorough understanding of the invention and for purposes of explanation and not limitation, specific details are set forth, such as a particular geometry of the deposition system and descriptions of various components. However, it should be understood that the invention may be practiced in other embodiments that depart from these specific details.
Referring now to the drawings,
The PEALD system 1 comprises a process chamber 10 having a substrate holder 20 configured to support a substrate 25, upon which the thin TaC or TaCN film is formed. The process chamber 10 further comprises an upper assembly 30 coupled to a first process material supply system 40, a second process material supply system 42, and a purge gas supply system 44. Additionally, the PEALD system 1 includes a first power source 50 coupled to the process chamber 10 and configured to generate plasma in the process chamber 10, and a substrate temperature control system 60 coupled to substrate holder 20 and configured to elevate and control the temperature of substrate 25. Additionally, the PEALD system 1 includes a controller 70 that can be coupled to process chamber 10, substrate holder 20, upper assembly 30, first process material supply system 40, second process material supply system 42, purge gas supply system 44, first power source 50, and substrate temperature control system 60.
Alternatively, or in addition, controller 70 can be coupled to one or more additional controllers/computers (not shown), and controller 70 can obtain setup and/or configuration information from an additional controller/computer.
In
The controller 70 can be used to configure any number of processing elements (10, 20, 30, 40, 42, 44, 50, and 60), and the controller 70 can collect, provide, process, store, and display data from processing elements. The controller 70 can comprise a number of applications for controlling one or more of the processing elements. For example, controller 70 can include a graphic user interface (GUI) component (not shown) that can provide easy to use interfaces that enable a user to monitor and/or control one or more processing elements.
Still referring to
The first process material supply system 40 and the second process material supply system 42 are configured to alternately introduce a first process material to process chamber 10 and a second process material to process chamber 10. The alternation of the introduction of the first material and the introduction of the second material can be cyclical, or it may be acyclical with variable time periods between introduction of the first and second materials. The first process material can, for example, comprise a TaC or TaCN film precursor, such as a composition having the principal atomic or molecular species found in the TaC or TaCN film formed on substrate 25. For instance, the TaC or TaCN film precursor can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 10 in a gaseous phase with or without the use of a carrier gas. The second process material can, for example, comprise a reducing agent, which may also include atomic or molecular species found in the film formed on substrate 25. For instance, the reducing agent can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 10 in a gaseous phase with or without the use of a carrier gas.
Additionally, the purge gas supply system 44 can be configured to introduce a purge gas to process chamber 10. For example, the introduction of purge gas may occur between introduction of the first process material and the second process material to process chamber 10, or following the introduction of the second process material to process chamber 10, respectively. The purge gas can comprise an inert gas, such as a noble gas (i.e., helium, neon, argon, xenon, krypton), or nitrogen (N2), or hydrogen (H2).
Referring still to
Alternatively, the first power source 50 may include a RF generator and an impedance match network, and may further include an antenna, such as an inductive coil, through which RF power is coupled to plasma in process chamber 10. The antenna can, for example, include a helical or solenoidal coil, such as in an inductively coupled plasma source or helicon source, or it can, for example, include a flat coil as in a transformer coupled plasma source.
Alternatively, the first power source 50 may include a microwave frequency generator, and may further include a microwave antenna and microwave window through which microwave power is coupled to plasma in process chamber 10. The coupling of microwave power can be accomplished using electron cyclotron resonance (ECR) technology, or it may be employed using surface wave plasma technology, such as a slotted plane antenna (SPA), as described in U.S. Pat. No. 5,024,716, entitled “Plasma processing apparatus for etching, ashing, and film-formation”; the contents of which are herein incorporated by reference in its entirety.
According to one embodiment of the invention, the PEALD system 1 includes a substrate bias generation system configured to generate or assist in generating a plasma (through substrate holder biasing) during at least a portion of the alternating introduction of the first process material and the second process material to process chamber 10. The substrate bias system can include a substrate power source 52 coupled to the process chamber 10, and configured to couple power to substrate 25. The substrate power source 52 may include a RF generator and an impedance match network, and may further include an electrode through which RF power is coupled to substrate 25. The electrode can be formed in substrate holder 20. For instance, substrate holder 20 can be electrically biased at a RF voltage via the transmission of RF power from a RF generator (not shown) through an impedance match network (not shown) to substrate holder 20. A typical frequency for the RF bias can range from about 0.1 MHz to about 100 MHz, and can be 13.56 MHz. RF bias systems for plasma processing are well known to those skilled in the art. Alternatively, RF power is applied to the substrate holder electrode at multiple frequencies.
Although the plasma generation system and the substrate bias system are illustrated in
Still referring to
In order to improve the thermal transfer between substrate 25 and substrate holder 20, substrate holder 20 can include a mechanical clamping system, or an electrical clamping system, such as an electrostatic clamping system, to affix substrate 25 to an upper surface of substrate holder 20. Furthermore, substrate holder 20 can further include a substrate backside gas delivery system configured to introduce gas to the back-side of substrate 25 in order to improve the gas-gap thermal conductance between substrate 25 and substrate holder 20. Such a system can be utilized when temperature control of the substrate is required at elevated or reduced temperatures. For example, the substrate backside gas system can comprise a two-zone gas distribution system, wherein the helium gas gap pressure can be independently varied between the center and the edge of substrate 25.
Furthermore, the process chamber 10 is further coupled to a pressure control system 32, including a vacuum pumping system 34 and a valve 36, through a duct 38, wherein the pressure control system 34 is configured to controllably evacuate the process chamber 10 to a pressure suitable for forming the thin film on substrate 25, and suitable for use of the first and second process materials. The vacuum pumping system 34 can include a turbo-molecular vacuum pump (TMP) or a cryogenic pump capable of a pumping speed up to about 5000 liters per second (and greater) and valve 36 can include a gate valve for throttling the chamber pressure. In conventional plasma processing devices utilized for dry plasma etch, a 300 to 5000 liter per second TMP is generally employed. Moreover, a device for monitoring chamber pressure (not shown) can be coupled to the processing chamber 10. The pressure measuring device can be, for example, a Type 628B Baratron absolute capacitance manometer commercially available from MKS Instruments, Inc. (Andover, Mass.).
Still referring to
However, the controller 70 may be implemented as a general purpose computer system that performs a portion or all of the microprocessor based processing steps of the invention in response to a processor executing one or more sequences of one or more instructions contained in a memory. Such instructions may be read into the controller memory from another computer readable medium, such as a hard disk or a removable media drive. One or more processors in a multi-processing arrangement may also be employed as the controller microprocessor to execute the sequences of instructions contained in main memory. In alternative embodiments, hard-wired circuitry may be used in place of or in combination with software instructions. Thus, embodiments are not limited to any specific combination of hardware circuitry and software.
The controller 70 includes at least one computer readable medium or memory, such as the controller memory, for holding instructions programmed according to the teachings of the invention and for containing data structures, tables, records, or other data that may be necessary to implement the present invention. Examples of computer readable media are compact discs, hard disks, floppy disks, tape, magneto-optical disks, PROMs (EPROM, EEPROM, flash EPROM), DRAM, SRAM, SDRAM, or any other magnetic medium, compact discs (e.g., CD-ROM), or any other optical medium, punch cards, paper tape, or other physical medium with patterns of holes, a carrier wave (described below), or any other medium from which a computer can read.
Stored on any one or on a combination of computer readable media, the present invention includes software for controlling the controller 70, for driving a device or devices for implementing the invention, and/or for enabling the controller to interact with a human user. Such software may include, but is not limited to, device drivers, operating systems, development tools, and applications software. Such computer readable media further includes the computer program product of the present invention for performing all or a portion (if processing is distributed) of the processing performed in implementing the invention.
The computer code devices of the present invention may be any interpretable or executable code mechanism, including but not limited to scripts, interpretable programs, dynamic link libraries (DLLs), Java classes, and complete executable programs. Moreover, parts of the processing of the present invention may be distributed for better performance, reliability, and/or cost.
The term “computer readable medium” as used herein refers to any medium that participates in providing instructions to the processor of the controller 70 for execution. A computer readable medium may take many forms, including but not limited to, non-volatile media, volatile media, and transmission media. Non-volatile media includes, for example, optical, magnetic disks, and magneto-optical disks, such as the hard disk or the removable media drive. Volatile media includes dynamic memory, such as the main memory. Moreover, various forms of computer readable media may be involved in carrying out one or more sequences of one or more instructions to processor of controller for execution. For example, the instructions may initially be carried on a magnetic disk of a remote computer. The remote computer can load the instructions for implementing all or a portion of the present invention remotely into a dynamic memory and send the instructions over a network to the controller 70.
The controller 70 may be locally located relative to the PEALD system 1, or it may be remotely located relative to the PEALD system 1. For example, the controller 70 may exchange data with the PEALD system 1 using at least one of a direct connection, an intranet, the Internet and a wireless connection. The controller 70 may be coupled to an intranet at, for example, a customer site (i.e., a device maker, etc.), or it may be coupled to an intranet at, for example, a vendor site (i.e., an equipment manufacturer). Additionally, for example, the controller 70 may be coupled to the Internet. Furthermore, another computer (i.e., controller, server, etc.) may access, for example, the controller 70 to exchange data via at least one of a direct connection, an intranet, and the Internet. As also would be appreciated by those skilled in the art, the controller 70 may exchange data with the deposition system 1 via a wireless connection.
Referring now to
The PEALD system 101 may be configured to process 200 mm substrates, 300 mm substrates, or larger-sized substrates. In fact, it is contemplated that the deposition system may be configured to process substrates, wafers, or LCDs regardless of their size, as would be appreciated by those skilled in the art. Substrates can be introduced to process chamber 110 through passage 112, and they may be lifted to and from an upper surface of substrate holder 120 via substrate lift system 122.
The first process material supply system 140 and the second process material supply system 142 are configured to alternately introduce a first process material to process chamber 110 and a second process material to process chamber 110. The alternation of the introduction of the first material and the introduction of the second material can be cyclical, or it may be acyclical with variable time periods between introduction of the first and second materials. The first process material can, for example, comprise a TaC or TaCN film precursor, such as a composition having the principal atomic or molecular species found in the film formed on substrate 125. For instance, the film precursor can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 110 in a gaseous phase, and with or without a carrier gas. The second process material can, for example, comprise a reducing agent, which may also have atomic or molecular species found in the film formed on substrate 125. For instance, the reducing agent can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 110 in a gaseous phase, and with or without a carrier gas.
According to one embodiment of the invention, the first process material and the second process material are chosen in accordance with the elemental composition and characteristics of the TaCN film to be deposited on the substrate. The first process material can include a Ta organic film precursor containing a “Ta—N—C” structural unit, such as tertiary amyl imido-tris-dimethylamido tantalum (Ta(NC(CH3)2C2H5)(N(CH3)2)3, hereinafter referred to as TAIMATA®; for additional details, see U.S. Pat. No. 6,593,484, the entire contents of which is incorporated herein by reference). In another example, the first process material can include (pentakis(diethylamido)tantalum (Ta[N(C2H5)2]5, PDEAT), pentakis(ethylmethylamido)tantalum (Ta[N(C2H5CH3)]5, PEMAT), pentakis(dimethylamido)tantalum (Ta[N(CH3)2]5, PDMAT), (t-butylimino tris(diethylamino)tantalum (Ta(NC(CH3)3)(N(C2H5)2)3, TBTDET), Ta(NC2H5)(N(C2H5)2)3, Ta(NC(CH3)2C2H5)(N(CH3)2)3, Ta(NC(CH3)3)(N(CH3)2)3, or tert-butyl-tris-ethylmethylamido tantalum ((CH3)3CNTa(NC2H5(CH3)3)3), TBTEMAT).
According to an embodiment of the invention, the second process material can include a reducing agent, such as hydrogen (H2) gas, ammonia (NH3), N2H4, NH(CH3)2, N2H3CH3, silane (SiH4), or disilane (Si2H6), or a combination of more than one thereof.
Additionally, the purge gas supply system 144 can be configured to introduce a purge gas to process chamber 110. For example, the introduction of purge gas may occur between introduction of the first process material and the second process material to process chamber 110, or following the introduction of the second process material to process chamber 110, respectively. The purge gas can comprise an inert gas, such as a noble gas (i.e., helium, neon, argon, xenon, krypton), or nitrogen (N2), or hydrogen (H2).
The first material supply system 140, the second material supply system 142, and the purge gas supply system 144 can include one or more material sources, one or more pressure control devices, one or more flow control devices, one or more filters, one or more valves, or one or more flow sensors. As discussed with respect to
Referring still to
Referring still to
According to one embodiment of the invention, the PEALD system 101 includes a substrate bias generation system configured to generate or assist in generating a plasma (through substrate holder biasing) during at least a portion of the alternating introduction of the first process material and the second process material to process chamber 110. The substrate bias system can include a substrate power source 152 coupled to the process chamber 110, and configured to couple power to substrate 125. The substrate power source 152 may include a RF generator and an impedance match network, and may further include an electrode 162 through which RF power is coupled to substrate 125. The electrode 162 can be formed in substrate holder 120. For instance, substrate holder 120 can be electrically biased at a RF voltage via the transmission of RF power from a RF generator (not shown) through an impedance match network (not shown) to substrate holder 120. A typical frequency for the RF bias can range from about 0.1 MHz to about 100 MHz. RF bias systems for plasma processing are well known to those skilled in the art. Alternatively, RF power is applied to the substrate holder electrode at multiple frequencies.
Still referring to
Furthermore, the process chamber 110 is further coupled to a pressure control system 132, including a vacuum pumping system 134 and a valve 136, through a duct 138, wherein the pressure control system 132 is configured to controllably evacuate the process chamber 110 to a pressure suitable for forming the thin film on substrate 125, and suitable for use of the first and second process materials.
Still referring to
According to embodiments of the invention, introduction of the first process material, purge, introduction of the second process material in the presence of plasma, and purge, may be repeated a desired number of times before the substrate 25/125 is exposed to plasma excited Argon gas. For example, the steps of introducing the first process material, purging, introducing the second process material in the presence of plasma, and purging, may be performed between 2 and 100 times, or between 30 and 70 times, prior the exposing the substrate 25/125 to plasma excited Argon. Furthermore, according to an embodiment of the invention, a process sequence that includes introducing the first process material, purging, introducing the second process material in the presence of plasma, and purging, repeated a desired number of times, followed by exposing the substrate 25/125 to plasma excited Argon, may be repeated any number of times. For example, the process sequence may be repeated between 1 and 100 times, or between 10 and 20 times, to produce a TaC or TaCN film with a desired thickness on the substrate 25/125.
Although the second process material time period 330 and the plasma time period 340 are shown in
Reference will now be made to
In step 404, the substrate 25/125 is exposed to a first process material containing tantalum in the absence of a plasma for a time period 310. As noted above, in some embodiments of the invention, a plasma may be generated during introduction of the first process material. The first process material can be a chemically volatile but thermally stable material that can be deposited on the substrate surface in a self limiting manner. The first process material can include TAIMATA, PDEAT, PEMAT, PDMAT, TBTDET, Ta(NC2H5)(N(C2H5)2)3, Ta(NC(CH3)2C2H5)(N(CH3)2)3, or Ta(NC(CH3)3)(N(CH3)2)3 for depositing a TaCN film. Alternatively, the first process material can include Ta(η5-C5H5)2H3, Ta(CH2)(CH3)(η5-C5)2, Ta(η3-C3H5)(η5-C5H5)2, Ta(CH3)3(η5-C5H5)2, Ta(CH3)4(η5-C5(CH3)5), or Ta(η5-C5(CH3)5)2H3 for depositing a TaC film. The first process material may be delivered “neat” (undiluted by a carrier gas) to the process chamber or a carrier gas may be used to dilute the first process material. The carrier gas can, for example, include Argon or N2. According to one embodiment of the invention, the first process material can be undiluted TAIMATA that is vaporized from TAIMATA liquid.
In step 406, the process chamber is purged of the first process material for a time period 320a. The purge step 406 allows the first process material to be exhausted from the PEALD process chamber by vacuum pumping prior to introduction of the second process material. The purging may include flowing a purge gas, for example Ar or N2, into the process chamber.
In step 408, the substrate is exposed to a second process material comprising a plasma excited reducing agent. According to an embodiment of the invention, the reducing agent can include hydrogen (H2) gas, ammonia (NH3), N2H4, NH(CH3)2, N2H3CH3, silane (SiH4), or disilane (Si2H6), or a combination of more than one thereof. The second process material may be delivered undiluted to the process chamber or a carrier gas may be used to dilute the second process material. The carrier gas can, for example, include Argon or N2. According to one embodiment of the invention, the reducing agent can be undiluted H2.
In step 408, the plasma excitation of the second process material heats the reducing agent, thus causing ionization and/or dissociation of the reducing agent in order to form radicals and/or ions that chemically react with the first precursor adsorbed on the substrate to facilitate the reduction process and reduce impurities within the deposited film. In an embodiment of the invention, the substrate holder bias can be between 100 W and 2000 W, or between 100 W and 500 W, while the upper assembly (electrode) 30,130 is grounded. However, the actual substrate holder bias may vary depending on factors such as the composition and characteristics of the TaC or TaCN film to be deposited. Suitable high power levels that enable PEALD deposition of a TaC or TaCN film at improved deposition speeds and with reduced impurities in accordance with an embodiment of the invention can be determined by direct experimentation and/or design of experiments (DOE). Other adjustable process parameters such as substrate temperature, process pressure, type of first and second process materials and relative gas flows can also be determined by direct experimentation and/or design of experiments (DOE).
In step 410, the process chamber is purged of the second process material for a time period 320b. The purging may include flowing a purge gas, for example Ar or N2, into the process chamber. Similarly, where multiple PEALD cycles are executed, a purge gas can be introduced after the reduction reaction takes place to expel the second process material before introduction of the first process material. This purging ensures that the reduction reaction occurs primarily at the adsorbed layer of the first process material on the substrate, rather than in the process chamber atmosphere prior to being deposited.
The reduction reaction completed by step 408 results in a thin layer of a TaC or TaCN being deposited on the substrate surface. The thin layer can have a thickness of about one atomic layer, or less. Once the reduction reaction takes place, steps 404, 406, 408, 410 can be repeated a desired number of times as shown by process flow 407 to deposit additional TaC or TaCN layers of the substrate.
In step 412, the TaC or TaCN layers from steps 404, 406, 408, 410, repeated a desired number of times, is exposed to plasma excited Argon for a time period 350. The present inventors have recognized that the PEALD process described in
In a preferred embodiment, the Argon plasma step 412 is performed within the process chamber as shown by
According one embodiment of the invention, at least one of steps 408 and 412 include applying substrate holder bias between 100 W and 2000 W, or between 100 W and 500 W.
Next, the TaC or TaCN film deposition may be repeated a desired number of times as shown by process flow 409 to deposit a TaC or TaCN film with a desired thickness. For example, the TaC or TaCN film can have a thickness between 1 nm and 20 nm, between 1 nm and 10 nm, or between 1 nm and 5 nm. According to one embodiment of the invention, the TaC or TaCN film can have a thickness of about 3 nm.
As seen in
The adhesion and agglomeration of Cu layers to TaCN films deposited according to embodiments of the invention was also measured. TaCN films of approximately 3 nm were deposited using 51 exposure cycles (one cycle includes steps 404, 406, 408, 410) at substrate temperature of 240° C., and using 40 exposure cycles at substrate temperature of 170° C., each with a substrate holder bias of 500 W in step 408. Each TaCN film was then exposed once to plasma excited Ar (step 412), using an Argon flow of 1,000 sccm, an exposure time of 60 sec, a process chamber pressure of 0.5 Torr, and a substrate holder bias of 100 W, 300 W, or 500 W. Next, a 10 nm thick Cu layer was deposited on the TaCN films by i-PVD. Subsequently, the substrate was annealed for 30 min at a substrate temperature of 400° C. in the presence of 10 Torr of Argon to evaluate the adhesion properties of the TaCN films to Cu. The annealing showed that TaCN films deposited at 170° C. and exposed to plasma excited Argon at a substrate holder bias of 100 W had improved adhesion to Cu, as shown by lack of Cu agglomeration visible by scanning electron microscopy (SEM). Furthermore, TaCN films deposited at 240° C. and exposed to plasma excited Argon at substrate holder bias of 500 W had improved adhesion to Cu.
Although only certain exemplary embodiments of inventions have been described in detail above, those skilled in the art will readily appreciate that many modifications are possible in the exemplary embodiments without materially departing from the novel teachings and advantages of this invention. Accordingly, all such modifications are intended to be included within the scope of this invention.
Number | Name | Date | Kind |
---|---|---|---|
6593484 | Yasuhara et al. | Jul 2003 | B2 |
7186446 | Kim et al. | Mar 2007 | B2 |
20020192952 | Itoh et al. | Dec 2002 | A1 |
20060210723 | Ishizaka | Sep 2006 | A1 |
20060211223 | Brcka | Sep 2006 | A1 |
20060211224 | Matsuda | Sep 2006 | A1 |
20060211243 | Ishizaka et al. | Sep 2006 | A1 |
20060211246 | Ishizaka et al. | Sep 2006 | A1 |
20060213437 | Ishizaka et al. | Sep 2006 | A1 |
20060213439 | Ishizaka | Sep 2006 | A1 |
Number | Date | Country | |
---|---|---|---|
20070218670 A1 | Sep 2007 | US |