Embodiments of the invention generally relate to systems for depositing materials on substrates, and to methods of making and using such systems. More particularly, embodiments of the invention relate to atomic layer deposition (ALD) methods for depositing III-V semiconductor materials on substrates and to methods of making and using such systems.
III-V semiconductor materials are rapidly developing for use in electronic and optoelectronic applications. Many III-V semiconductor materials have direct band gaps, which make them particularly useful for fabricating optoelectronic devices, such as light-emitting diodes (LEDs) and laser diodes (LDs). Specific III-V semiconductor materials, such as gallium nitride (GaN), indium nitride (InN), aluminum nitride (AlN) and their alloys (commonly referred to as the III-nitrides), are emerging as important materials for the production of shorter wavelength LEDs and LDs, including blue and ultra-violet light-emitting optoelectronic devices. Wide band gap III-nitrides may also be utilized for high-frequency and high-power electronic devices due to the III-nitrides' ability to operate at high current levels, high breakdown voltages and high temperatures.
One widely used process for depositing III-V semiconductor materials is referred to in the art as metal-organic chemical vapor deposition (MOCVD). In MOCVD processes, a substrate is exposed to one or more gaseous precursors in a reaction chamber, which react, decompose, or both react and decompose in a manner that results in the epitaxial deposition of the group III-V material on a surface of the substrate. MOCVD processes are often used to deposit III-V semiconductor materials by introducing both a precursor containing a group III element (i.e., a group III element precursor) and a precursor containing a group V element (i.e., a group V element precursor) into the reaction chamber containing the substrate. This results in mixing of the precursors (i.e., the group III element precursor and the group V element precursor) before their exposure to the surface of the substrate.
Deposition of III-V semiconductor materials using a MOCVD process involves a balance between growth rate at the surface of the substrate and compound formation in the vapor phase. Specifically, mixing of the group III element precursor and the group V element precursor may result in the formation of particles that consume the precursors that are otherwise used to form the III-V semiconductor material on a suitable growth substrate. Consumption of available precursors during the MOCVD process creates difficulties in controlling the growth rate, thickness and composition of the III-V semiconductor material, especially in large reaction chambers. Variation in the thickness and composition of the III-V semiconductor material formed using the MOCVD processes may negatively affect throughput and yield of devices having a specific emission wavelength, such as wavelength-specific LEDs. Furthermore, deposition rates of III-V semiconductor materials formed by MOCVD processes are generally low, thus decreasing throughput and increasing cost per wafer.
Atomic layer deposition (ALD) is a process used to deposit conformal material with atomic scale thickness control. ALD may be used to deposit III-V semiconductor materials. ALD is a multi-step, self-limiting process that includes the use of at least two reagents or precursors. Generally, a first precursor is introduced into a reactor containing a substrate and adsorbed onto a surface of the substrate. Excess precursor may be removed by pumping and purging the reactor using, for example, a purge gas. A second precursor is then introduced into the reactor and reacted with the adsorbed material to form a conformal layer or film of a material on the substrate. Under select growth conditions the deposition reaction may be self-limiting in that the reaction terminates once the initially adsorbed material reacts fully with the second precursor. Excess precursor is again removed by pumping and purging the reactor. The process may be repeated to form another layer of the material, with the number of cycles determining the total thickness of the deposited film.
III-V semiconductor materials formed utilizing ALD processes may be of a higher crystalline quality than those formed by conventional MOCVD processes. ALD processes may allow for greater control of precursor incorporation into the deposited crystalline material and consequently a greater control of the composition of the crystalline material formed, e.g., of the III-V semiconductor material formed by such ALD processes. Such stringent control of the composition of the III-V semiconductor material may be of consequence in light-emitting devices, for example, to ensure a uniform emission wavelength between light-emitting devices fabricated on a single growth substrate and between light-emitting devices from growth substrate to growth substrate.
However, the growth rate of III-V semiconductor materials by conventional ALD processes is relatively low in comparison to that of MOCVD. Furthermore, high throughput of III-V semiconductor materials by conventional ALD requires increased load sizes that make purging excess precursor and purge gas out of the reactor difficult. Thus, currently available ALD reactors are often configured for single wafer processing, leading to low throughput and high cost per wafer of III-V semiconductor materials by ALD.
Recently, ALD methods and systems have been developed in which each precursor is provided continuously in spatially separated regions, and each precursor is introduced to the substrate as the substrate is moved through each precursor in succession. Such processes are often referred to in the art as “spatial ALD” or “S-ALD.”
This summary is provided to introduce a selection of concepts in a simplified form, such concepts being further described in the detailed description below of some example embodiments of the invention. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
In some embodiments, the present invention includes method of depositing material, such as a III-V semiconductor material, on a substrate. A group III element precursor and a group V element precursor may be introduced into alternating gas injectors of a plurality of substantially aligned gas injectors. A substrate may be moved relative to the plurality of substantially aligned gas injectors such that a surface of the substrate is exposed to the group III element precursor and the group V element precursor forming at least one III-V semiconductor material on the surface of the substrate.
In additional embodiments, the present invention includes deposition systems for forming semiconductor materials. The deposition systems may include a manifold including a plurality of substantially aligned gas injectors and at least one assembly for moving a substrate along a length of the manifold. At least one of the plurality of substantially aligned gas injectors includes an inlet, a thermalizing conduit, a liquid container configured to hold a liquid reagent therein, and an outlet. A pathway extends from the inlet, through the thermalizing conduit to an interior space within the liquid container, and from the interior space within the liquid container to the outlet.
The present invention may be understood more fully by reference to the following detailed description of example embodiments of the present invention, which are illustrated in the appended figures in which:
The illustrations presented herein are not meant to be actual views of any particular component, device, or system, but are merely idealized representations that are employed to describe embodiments of the present invention.
A number of references are cited herein, and the disclosures of which are incorporated herein, in their entireties, by this reference for all purposes. Further, none of the cited references, regardless of how characterized herein, are admitted as prior art relative to the invention of the subject matter claimed herein.
As used herein, the term “III-V semiconductor material” means and includes any semiconductor material that is at least predominantly comprised of one or more elements from group IIIA of the periodic table (B, Al, Ga, and In) and one or more elements from group VA of the periodic table (N, P, As and Sb). For example, III-V semiconductor materials include, but are not limited to, gallium nitride, gallium phosphide, gallium arsenide, indium nitride, indium phosphide, indium arsenide, aluminum nitride, aluminum phosphide, aluminum arsenide, indium gallium nitride, indium gallium phosphide, indium gallium arsenide, aluminum gallium nitride, aluminum gallium phosphide, aluminum gallium arsenide, indium gallium nitride phosphide, etc.
As used herein, the term “gas” includes gases (fluids that have neither independent shape nor volume) and vapors (gases that include diffused liquid or solid matter suspended therein), and the terms “gas” and “vapor” are used synonymously herein.
As used herein, the term “ALD growth cycle” means and includes exposing a surface of a substrate to a first precursor, chemisorption of the first precursor onto the surface of the substrate, exposing the surface of the substrate to a second precursor, and a surface reaction to form a layer of material.
Methods and systems that utilize an external source of one or more metal halides, such as, for example, gallium trichloride (GaCl3), indium trichloride (InCl3), and/or aluminum trichloride (AlCl3) as precursors have recently been developed. Examples of such methods and systems are disclosed in U.S. Patent Application Publication No. US 2009/0223442 A1, which published Sep. 10, 2009 in the name of Arena et al., the entire disclosure of which application is incorporated herein in its entirety by this reference. Further, improved gas injectors have also been recently developed for use in such methods and systems. Examples of such gas injectors are disclosed in, for example, U.S. Provisional Patent Application Ser. No. 61/157,112, which was filed on Mar. 3, 2009 in the name of Arena et al., and in U.S. patent application Ser. No. 12/894,724, which was filed Sep. 30, 2010 in the name of Ronald T. Bertran, Jr. and entitled “Thermalizing Gas Injectors for Generating Increased Precursor Gas, Material Deposition Systems Including Such Injectors, and Related Methods,” the entire disclosure of each of which application is incorporated herein in its entirety by this reference.
The metal halides are classified as inorganic ALD precursors. The use of such inorganic metal halide precursors for ALD processes may be advantageous over, for example, organic precursors since they are generally smaller, more reactive, thermally stable and usually leave small amounts of ligand residues in the deposited crystalline material. Small ligands reduce the risk of steric hindrance and, as a result, reduce growth per cycle. High thermal stability enables deposition without thermal decomposition at higher temperatures.
Embodiments of the present invention include, and make use of, new gas injectors in an atomic layer deposition (ALD) process, as described in further detail below. An example of an embodiment of a deposition system 100 of the invention that includes a plurality of gas injectors 102A, 102B, 102C, 102D, such as those described in U.S. Provisional Patent Application Ser. No. 61/157,112 or U.S. patent application Ser. No. 12/894,724 is described below with reference to
The deposition system 100 may further include a manifold 104 and an assembly 106, such as a track, a conveyor or a support. The manifold 104 may include a plurality of gas columns 108 configured to receive at least one gas through a port 110 therein. The gas columns 108 may be positioned in longitudinal alignment with one another to form the manifold 104. The gas columns 108 of the manifold 104 may be arranged in any suitable configuration, such as a linear, a folded or a serpentine configuration. In some embodiments, the manifold 104 is configured to move relative to one or more workpiece substrates 112 (e.g., one or more dies or wafers) on which it is desired to deposit or otherwise provide III-V semiconductor material, as indicated by directional arrow 103. In other embodiments, the assembly 106 is configured to move the workpiece substrate 112 relative to the gas columns 108 of the manifold 104, as indicated by directional arrow 105. For example, the workpiece substrates 112 may comprise dies or wafers. The gas columns 108 may, therefore, be positioned at a sufficient distance above the assembly 106 for the workpiece substrate 112 to be moved through a space between the gas columns 108 and the assembly 106.
In the following description of the deposition system 100 and, more particularly, the manifold 104 of the deposition system 100, the terms “longitudinal” and “transverse” are used to refer to the directions relative to the manifold 104 and the assembly 106 and as shown in
In some embodiments, the deposition system 100 includes a gas flow system used to supply one or more gases into the manifold 104 and to remove gases out of the manifold 104. For example, the deposition system 100 may include gas sources 114A, 114B, 114C, 114D that supply the gases to respective gas injectors 102A, 102B, 102C, 102D.
For example, one or more of the gas sources 114A, 114B, 114C, 114D may comprise an external source of a group III element or a group V element that may be supplied to the gas injectors 102A, 102B, 102C, 102D. The group III element source may include at least one of a source of gallium (Ga), a source of indium (In) and a source of aluminum (Al). As a non-limiting example, the group III element source may comprise at least one of gallium trichloride (GaCl3), indium trichloride (InCl3) and aluminum trichloride (AlCl3). The group III element source, comprising at least one of GaCl3, InCl3 or AlCl3, may be in the faun of a dimer such as, for example, Ga2Cl6, In2Cl6 or Al2Cl6. The group V element source may include a source of nitrogen (N), a source of arsenic (As) and/or a source of phosphorus (P). By way of example and not limitation, the group V element source may comprise one or more of ammonia (NH3), arsine (AsH3) or phosphine (PH3). In some embodiments, source gases may be supplied from the gas sources 114A, 114B, 114C, 114D to the gas injectors 102A, 102B, 102C, 102D using one or more carrier gases, such as hydrogen gas (H2), helium gas (He), argon (Ar), etc. The source gas may therefore comprise one or more group III element sources as well as one or more carrier gases.
As the source gas is conveyed from the gas sources 114A, 114B, 114C, 114D through conduits 116, the source gas may be heated to a temperature sufficient to generate a precursor gas from the source gas. For example, the source gas may include GaCl3 and H2, which may be heated to a temperature sufficient for the gallium trichloride to dissociate in the presence of hydrogen into gallium chloride (GaCl) and a chlorinated species, such as hydrogen chloride gas (HCl) and/or chlorine gas (Cl2).
The gas sources 114A, 114B, 114C, 114D may supply source gas to the gas injectors 102A, 102B, 102C, 102D. Each of the gas injectors 102A, 102B, 102C, 102D may be configured for generating one or more precursors and for introducing the precursors to the workpiece substrate 112. For example, the gas injectors 102A, 102B, 102C, 102D may be configured to supply precursor gases to the elongated gas columns 108, which may be configured to direct the precursor gases toward the major surface of the workpiece substrate 112 in a direction substantially perpendicular to the major surface of the workpiece substrate 112. Thus, an area on the assembly 106 underlying each of the gas columns 108 represents an injection point at which the workpiece substrate 112 is exposed to the precursor gases.
The gas injectors 102A, 102B, 102C, 102D may each operate independently and may be spaced from adjacent gas injectors 102A, 102B, 102C, 102D at a distance sufficient to prevent cross-contamination of gases released by adjacent injectors 102A, 102B, 102C, 102D. Each of the gas injectors 102A, 102B, 102C, 102D may be configured to provide a sufficient amount of gas to saturate a surface of the workpiece substrate 112 and deposit a layer of a material on the surface of the workpiece substrate 112. The manifold 104 of the deposition system 100 shown in
In embodiments where the group III element precursor is formed from a gas comprising GaCl3, InCl3, or AlCl3, the group III element precursor may be formed from the gas using at least one of the gas injectors 102A, 102B, 102C, 102D, as will be described.
The deposition system 100 also includes features for maintaining separation of the precursor gases during deposition of the III-V semiconductor material. For example, the deposition system 100 may include at least one purge gas source 118 for supplying a purge gas to corresponding gas columns 108 and an exhaust line 120 for drawing excess precursor gases from the deposition system 100, as indicated by directional arrow 121. The purge gas source 118 may comprise a purge gas, such as argon (Ar), nitrogen (N2), and helium (He). The purge gas source 118 may be used to deliver the purge gas to the workpiece substrate 112 via the gas columns 108. For example, the purge gas source 118 may supply the purge gas to at least one of the gas columns 108 disposed between two of the gas columns 108 used to supply the precursors to the workpiece substrate 112. The gas columns 108 may also be used to remove excess gases (i.e., the precursor gases and the purge gases) from a surface of the workpiece substrate 112. The excess gases may be passed through the gas columns 108 and into the exhaust line 120 for removal from the deposition system 100. For example, the excess gases may be removed through one of the gas columns 108 disposed between each of the gas columns 108 configured to supply the precursor gases and purge gas to the workpiece substrate 112.
The assembly 106 is configured to support the workpiece substrate 112 and, in some embodiments, to transport the workpiece substrate 112 in sequence under each successive gas column 108. Although a single workpiece substrate 112 is shown in
As the workpiece substrate 112 is moved relative to the gas columns 108, a plurality of ALD growth cycles for forming a III-V semiconductor material over the surface of the workpiece substrate 112 may be completed.
As previously mentioned, one or more of the gas injectors 102A, 102B, 102C, 102D of the deposition system 100 may be or include one of the various embodiments of gas injectors described in detail with reference to
Furthermore, the thermalizing conduit 206 may include one or more curved sections or turns, such that the length of the physical space occupied by the thermalizing conduit 206 is significantly less than the actual length of the flow path through the thermalizing conduit 206. Stated another way, a length of the thermalizing conduit 206 may be longer than a shortest distance between the inlet 202 and the liquid container 210. In some embodiments, the length of the thermalizing conduit 206 may be at least about twice the shortest distance between the inlet 202 and the liquid container 210, at least about three times the shortest distance between the inlet 202 and the liquid container 210, or even at least about four times the shortest distance between the inlet 202 and the liquid container 210. For example, the thermalizing conduit 206 may have a serpentine configuration, as shown in
The thermalizing conduit 206 may comprise a tube that is at least substantially comprised of a refractory material such as, for example, quartz.
In some embodiments, the source gas may at least partially decompose within the thermalizing conduit 206. For example, in embodiments in which the source gas comprises GaCl3 and H2, the GaCl3 may decompose in the presence of H2 into gaseous GaCl and a chlorinated gas species, such as, for example, hydrogen chloride gas (HCl) and/or chlorine gas (Cl2).
The gases flow from the thermalizing conduit 206 into the container 210.
The interior space within the hollow container 210 may be partially filled with a liquid reagent, such as liquid gallium, liquid indium and liquid aluminum. For example, the container 210 may be filled with the liquid reagent to the level indicated by the dashed line 220 in
For example, in embodiments in which the source gas comprises GaCl3 and a carrier gas, such as H2, and the source gas has decomposed to include gaseous GaCl and a chlorinated gas species within the thermalizing conduit 206, the liquid reagent within the container 210 may comprise liquid gallium, which may react with the chlorinated gas species (e.g., HCl) generated within the thermalizing conduit 206 to form additional gaseous GaCl. Alternatively, the liquid reagent within the container 210 may comprise liquid indium or liquid aluminum, which may respectively react with the chlorinated gas species (e.g., HCl) to form InCl or AlCl. The gases within the space 222 over the liquid reagent within the container 210 may flow out from the container through an outlet port 228. For example, the outlet port 228 may be located in the top wall 214 of the container 210 over the horizontally extending portion of the tube 224. The outlet port 228 may lead to an outlet conduit 230, an end of which may define the outlet 204 of the gas injector 200 (
The various components of the container 210 may be at least substantially comprised of a refractory material such as, for example, quartz.
The GaCl may be a desirable precursor gas for forming GaN. Thus, by converting the excess chlorinated gas that results from thermal decomposition of GaCl3 (in systems that employ GaCl3 as a source gas) into additional GaCl, detrimental effects of excess chlorinated gas species to the deposited GaN material may be avoided, since the amount of chlorinated gas species introduced to the workpiece substrate 112 (
As shown in
The passive heating element 302 may be at least substantially comprised of materials with high emissivity values (close to unity) (black body materials) that are also capable of withstanding the high-temperature, corrosive environments that may be encountered within the deposition system 100 (
The passive heating element 302 may be solid or hollow. In some embodiments, the passive heating element 302 may be hollow, and a thermocouple may be positioned within the interior space of the passive heating element 302 for temperature monitoring and control purposes. In additional embodiments, a cylindrical thermocouple may be positioned around the passive heating element 302 and between the passive heating element 302 and the surrounding thermalizing conduit 206.
In additional embodiments, hollow cylindrical passive heating elements may be disposed over and around one or more straight sections of the thermalizing conduit 206. In such embodiments, a cylindrical thermocouple may be positioned between the hollow cylindrical passive heating elements and the sections of the thermalizing conduit 206 surrounded by the hollow cylindrical passive heating elements.
The thermalizing gas injector 300 also may include an active heating element 304. The active heating element 304 may at least partially surround each of the thermalizing conduit 206 and the container 210 of the gas injector 200. In some embodiments, the active heating element 304 may be generally cylindrical and may extend entirely around at least a portion of each of the thermalizing conduit 206 and the container 210, as shown in
The active and passive heating elements 304, 302 of the thermalizing gas injector 300 may be capable of heating the thermalizing conduit 206, the container 210 and the source gas to temperatures between about 500° C. and about 1,000° C.
As shown in
With continued reference to
The gas injector 500 also may include active and/or passive heating elements, such as, for example, the active heating element 304 and the insulating jacket 306 previously described in relation to the gas injector 300 of
A source gas, such as gaseous hydrogen chloride, chlorine or gaseous GaCl may be supplied from an external gas source to the inlet 202. The source gas may flow from the inlet 202 through the conduit 502 to the container 210, where the source gas may react with the metal reagent within the container 210 to form a precursor gas (e.g., InCl, AlCl, FeCl, etc.). The precursor gas may flow out from the container 210 through the outlet 204.
The flow rate of the gases through the gas injector 500 relative to the flow rates of the other gas injectors of the deposition system 100 may be selectively controlled so as to control the concentration of the elements deposited from the dopant precursor in the resulting III-V semiconductor material.
As described above, embodiments of thermalizing gas injectors of the invention may be used to inject gaseous group III element precursors and group V element precursors onto the workpiece substrate 112 for depositing III-V semiconductor materials using an S-ALD process. For example, in some embodiments, the thermalizing gas injectors of the invention may be used to convert GaCl3 into gaseous GaCl by thermal decomposition of GaCl3 in the presence of hydrogen, and by reaction of a chlorinated species (e.g., HCl, Cl2) resulting from such thermal decomposition of GaCl3 with liquid gallium, and to inject GaCl onto the workpiece substrate 112 for the deposition of GaN in an ALD process.
As shown in
Referring to
In a first branch 126A of the conduit 116, GaCl and at least one of hydrogen chloride and chlorine gas may be generated from one or more of GaCl3 and H2 using an injector 102 such as that described with respect to
In some embodiments, additional gases that may be used for doping the III-V semiconductor materials may be added to the conduits 116. As shown in
In additional embodiments shown in
The deposition system 100 described with respect to
At least one of the assembly 106 and the manifold 104 is configured to establish movement of the workpiece substrate 112 relative to the manifold 104. The workpiece substrate 112 may be positioned on the assembly 106 and moved relative to the manifold 104 through a series of injection positions along the length of the manifold 104 (i.e., positions underlying each of the longitudinally aligned gas injectors 102A, 102B, 102C, 102D). At each of the injection positions, the workpiece substrate 112 may be exposed to the at least one group III element precursor or the at least one group V element precursor by the overlying gas injector 102A, 102B, 102C, 102D such that a layer of a group III material, a group V material or a group III-V compound material is deposited on the workpiece substrate 112. The gas injectors 102A, 102B, 102C, 102D may be programmed to control the precursor flow rate and composition to form the desired III-V semiconductor material.
The group III element precursor may be formed from a group III element source using embodiments of the thermalizing gas injectors of the invention, which were previously described. In some embodiments, at least one of GaCl3, InCl3 and AlCl3 and one or more carrier gases, such as H2, N2 and Ar, may be thermalized using the gas injectors 102A, 102B, 102C, 102D to form the group III element precursor (i.e., GaCl, InCl and AlCl). In other embodiments, the group III element source including a mixture of gases, such as GaCl3, InCl3 and AlCl3, may be used to form ternary and quaternary III-V semiconductor materials, such as InGaN, InGaAs, InGaP, AlGaN, AlGaAs and AlGaP. For example, the mixture of gases may be formed prior to entry into the gas injectors 102A, 102B, 102C, 102D, as described with respect to
The group V element precursor may be formed by thermalizing a group V element source or by other techniques known in the art (e.g., plasma generation techniques). For example, at least one of ammonia (NH3), arsine (AsH3) and phosphine (PH3) may be thermalized to form the group V element precursor.
In some embodiments of the invention, one or more of the gas injectors 102A, 102B, 102C, 102D may be used to generate a group III element precursor, such as GaCl, InCl or AlCl, and to expose a major surface of the workpiece substrate 112 to the group III element precursor. In additional embodiments of the invention, one or more of the gas injectors 102A, 102B, 102C, 102D may be used to generate different group III element precursors that may be used to form group III nitride compound materials that include two or more different group III elements such as, for example, InGaN, AlGaN, InAlGaN, etc. By way of example and not limitation, first and third gas injectors 102A, 102C may be used to supply one or more of GaCl (by converting GaCl3 into gaseous GaCl by thermal decomposition of GaCl3, and by reaction of chlorinated species resulting from such thermal decomposition of GaCl3 with liquid gallium), InCl (by converting InCl3 into gaseous InCl by thermal decomposition of InCl3, and by reaction of chlorinated species resulting from such thermal decomposition of InCl3 with liquid indium) and AlCl (by converting AlCl3 into gaseous AlCl by thermal decomposition of AlCl3, and by reaction of chlorinated species resulting from such thermal decomposition of InCl3 with liquid indium), and second and fourth gas injectors 102B, 102D may be used to supply gaseous ammonia (NH3), gaseous arsine (AsH3), or gaseous phosphine (PH3). Each gas injector 102A, 102B, 102C, 102D may introduce a sufficient amount of precursor gas to the workpiece substrate 112 to deposit a layer of material on the workpiece substrate 112. The deposition system 100 may include any number of gas injectors 102A, 102B, 102C, 102D for depositing the desired thickness of the III-V semiconductor material or the plurality of layers of different III-V semiconductor materials on the workpiece substrate 112. In addition, the workpiece substrate 112 may be passed through the deposition system 100 any number of times to obtain a desirable thickness of the III-V semiconductor material or the plurality of layers of different III-V semiconductor materials.
In yet additional embodiments of the invention, at least one of the gas injectors 102A, 102B, 102C, 102D may be used to generate a dopant precursor (e.g., iron chloride (FeCl) or a vapor phase species comprising silicon (Si)) that may be used to introduce a dopant (e.g., iron atoms or ions or silicon atoms or ions) to the III-V semiconductor material. During the deposition process, the dopant precursor may decompose and/or react with another substance in such a manner as to result in the dopant being incorporated into the III-V semiconductor material being deposited. In such embodiments, it may not be necessary to thermally decompose the dopant precursor in the gas injector used to inject the dopant precursor.
By way of non-limiting example, each of the ALD growth cycles 122, 124 may be used to form a layer of the III-V semiconductor material having a desired composition or a plurality of layers of III-V semiconductor material, each having a different composition. A first ALD growth cycle 122 may be performed to deposit a first layer of III-V semiconductor material. As the workpiece substrate 112 moves along the length of the manifold 104 through a first ALD growth cycle 122, the workpiece substrate 112 may be positioned under the gas column 108 in communication with the first injector 102A. The first injector 102A may supply the group III element precursor to the workpiece substrate 112 through the corresponding gas column 108 and the group III element may be absorbed on the surface of the workpiece substrate 112.
Excess gases or group III element precursor may be removed from the workpiece substrate 112 by pumping the gases from the surface of the workpiece substrate 112 through the gas columns 108 connected to the exhaust line 120. A purging act may also be performed between pumping acts by exposing the surface of the workpiece substrate 112 to the purge gas.
The workpiece substrate 112 may then be moved relative to the manifold 104 to a position under the second injector 102B. The workpiece substrate 112 may be exposed to the group V element precursor supplied by the second injector 102B. The second injector 102B may introduce a sufficient amount of the group V element precursor to the workpiece substrate 112 that the group V element reacts with the group III element deposited on the surface of the workpiece substrate 112 by the first injector 102A to form the first layer of III-V semiconductor material. Excess gases or group V element precursor may be removed from the workpiece substrate 112 by pumping and purging, as previously described. The ALD growth cycle 122 may be repeated any number of times to increase a thickness of the first layer of III-V semiconductor material.
Another ALD growth cycle 124 may be performed to deposit a second layer of III-V semiconductor material having a composition different from that of the first layer of III-V semiconductor material. As the workpiece substrate 112 is moved relative to the manifold 104 through the second ALD growth cycle 124, the workpiece substrate 112 may be positioned under the third injector 102C. The third injector 102C may introduce the group III element precursor to the workpiece substrate 112 and the group III element may be absorbed on the surface of the workpiece substrate 112.
Excess gases or precursor may be removed from the workpiece substrate 112 by pumping and purging, as previously described.
After removing the excess gases, the workpiece substrate 112 may be moved relative to the manifold 104 to a position under the fourth injector 102D. The fourth injector 102D may introduce the group V element precursor to the workpiece substrate 112 and the group V element may react with the group III element deposited on the surface of the workpiece substrate 112 to form the second layer of III-V semiconductor material. The ALD growth cycle 124 may be repeated any number of times to increase a thickness of the second layer of III-V semiconductor material.
The thickness of the layer of III-V semiconductor material formed in one of the ALD growth cycles 122, 124 may depend on the precursors used and the speed of relative movement of the workpiece substrate 112 along the length of the manifold 104. Any number of ALD growth cycles 122, 124 may be performed to deposit a desired thickness of the III-V semiconductor material or to form layers of the III-V semiconductor materials having different compositions. The types of precursors introduced to the workpiece substrate 112 by the gas injectors 102A, 102B, 102C, 102D may be tailored to form the desired III-V semiconductor material or the desired plurality of layers of III-V semiconductor materials. In embodiments where a structure including a plurality of layers of III-V semiconductor materials is formed, the desired thickness of a specific III-V semiconductor material may be formed on the workpiece substrate 112 by performing one or more first ALD growth cycles 122 and, thereafter, one or more second ALD growth cycles 124 may be performed to form a desired thickness of another, different III-V semiconductor material. The ALD growth cycles 122,124 may be tailored to control the thickness and composition of each layer of III-V semiconductor material deposited using the deposition system 100.
Relative movement of the workpiece substrate 112 and the manifold 104 enables continuous, sequential exposure of the workpiece substrate 112 to different precursors without loading and unloading the workpiece substrate 112 from a reaction chamber between ALD growth cycles, as with conventional CVD systems, temperature ramps, cleaning, pump down, etc. The speed of the relative movement of the workpiece substrate 112 with respect to the manifold 104 may be varied according to a reaction time of the precursors, providing a high growth rate of the III-V semiconductor materials. The thickness and composition of each of the III-V semiconductor materials deposited may be determined by a number of injection positions (i.e., positions under each of the gas columns 108 corresponding to the gas injectors 102A, 102B, 102C, 102D) in the deposition system 100 and the type of precursors introduced to the workpiece substrate 112 at each of these injection positions. Thus, the deposition system 100 enables accurate control of the thickness and the composition of each of the III-V semiconductor materials. The deposition system 100 may be configured to deposit any combination of III-V semiconductor material layers, each having a desired thickness and composition. The deposition system 100, and related methods, further provide substantially increased throughput of III-V semiconductor materials in comparison to conventional deposition systems and methods, thus reducing fabrication costs. The deposition system 100 further enables fabrication of structures including multiple layers of III-V semiconductor materials, such as those used in III-nitride based devices, such as Laser Diode, LEDs, high-frequency and power diodes.
The following example serves to explain an embodiment of the present invention in more detail. This example is not to be construed as being exhaustive or exclusive as to the scope of this invention.
The deposition system 100 may be maintained at a temperature in a range of from about 350° C. to about 750° C. and a pressure in a range of from about 1000 mTorr to about 7600 mTorr. As a non-limiting example, gas sources may be supplied at a flow rate in a range of from about 1 sccm to about 100 sccm.
In some embodiments, the deposition system 100 may include a plurality of deposition zones 130A, 130B, 130C, 130D, 130E, 130F, each of which is used to form a structure including a plurality of layers on the workpiece substrate 112, each of the layers comprising a III-V semiconductor material having a specific composition. For example, the structure may be an LED device layer structure. In embodiments in which a structure including alternating layers of InGaN and GaN underlying a layer of doped p-type AlGaN and a layer of doped p-type GaN is formed, the deposition system 100 may include first and third deposition zones 130A, 130C for depositing an InGaN material, second and fourth deposition zones 130B, 130D for depositing a GaN material, a fifth deposition zone 130E for depositing a doped p-type AlGaN material and a sixth deposition zone 130F for depositing a doped p-type GaN material. As the workpiece substrate 112 is moved through the zones 130A, 130B, 130C, 130D, 130E, 130F of the deposition system 100, alternating exposures of an appropriate group III precursor and a nitrogen precursor may be introduced to the workpiece substrate 112 to form the desired III-V semiconductor material.
In some embodiments, a thickness of 1 nm of the desired III-V semiconductor material may be deposited every one (1) meter of the manifold 104. In embodiments in which the assembly 106 comprises a track or conveyor used to move the workpiece substrate 112 along a length of the manifold 104, the track may have a length of about 100 meters to move the workpiece substrate 112 under a sufficient number of gas injectors 102A, 102B, 102C, 102D to form a III-V semiconductor material, such as an LED device layer structure, having a thickness of 100 nm. The deposition system 100 may be arranged in a variety of configurations depending on available space. In embodiments where the deposition system has a processing rate of about 1000 wafers per hour, the track may be about 100 square meters (m2) and assuming a deliver rate of device layer structures of 1000 wafer per hour. This corresponds to an area per effective cycle time per wafer of about 0.1 m2 per wafer per hour, which is a substantial improvement over processing rates for conventional CVD reactors.
Additional non-limiting example embodiments of the invention are described below.
A method of depositing a semiconductor material, the method comprising: flowing a group III element precursor through a first gas column of a plurality of substantially aligned gas columns; flowing a group V element precursor through a second gas column of the plurality of substantially aligned gas columns; establishing movement of a substrate relative to the plurality of substantially aligned gas columns; and sequentially exposing a surface of the substrate to the group III element precursor and the group V element precursor to form a III-V semiconductor material.
The method of embodiment 1, further comprising decomposing a gas comprising at least one group III element to generate the group III element precursor.
The method of Embodiment 2, wherein decomposing a gas comprising at least one group III element to generate the group III element precursor comprises decomposing at least one of GaCl3, InCl3, and AlCl3 to form at least one of GaCl, InCl, and AlCl and chlorine.
The method of Embodiment 3, wherein decomposing at least one of GaCl3, InCl3, and AlCl3 to form at least one of GaCl, InCl, and AlCl and chlorine comprises decomposing GaCl3 to form GaCl and chlorine.
The method of Embodiment 2 or Embodiment 3, further comprising reacting the chlorine with liquid gallium to form additional GaCl.
The method of any one of Embodiments 1 through 5, further comprising increasing a thickness of the III-V semiconductor material by repeatedly exposing the surface of the substrate to the group III element precursor and the group V element precursor.
The method of any one of Embodiments 1 through 6, further comprising: flowing a purge gas through a third gas column disposed between the first gas column and the second gas column; and exposing the substrate to the purge gas to remove excess group III element precursor and excess group V element precursor from the surface of the substrate.
The method of any one of Embodiments 1 through 7, wherein sequentially exposing a surface of the substrate to the group III element precursor and the group V element precursor comprises: exposing the surface of the substrate to at least one of GaCl, InCl, and AlCl to absorb at least one of gallium, indium, and aluminum to the surface of the substrate; and exposing the at least one of gallium, indium, and aluminum absorbed on the surface of the substrate to at least one of nitrogen, arsenic, and phosphorous.
The method of any one of Embodiments 1 through 8, wherein sequentially exposing a surface of the substrate to the group III element precursor and the group V element precursor to form a III-V semiconductor material comprises forming at least one of gallium nitride, indium nitride, aluminum nitride, indium gallium nitride, indium gallium arsenide, indium gallium phosphide, aluminum gallium nitride, aluminum gallium arsenide, and aluminum gallium phosphide.
The method of any one of Embodiments 1 through 9, wherein sequentially exposing a surface of the substrate to the group III element precursor and the group V element precursor to a III-V semiconductor material comprises forming the III-V semiconductor material having a thickness of about 100 nm.
The method of any one of Embodiments 1 through 10, further comprising sequentially exposing a surface of the substrate to another group III element precursor and another group V element precursor to form another III-V semiconductor material over the III-V semiconductor material, the another III-V semiconductor material having a different composition than the III-V semiconductor material.
A method of depositing a semiconductor material, comprising: thermally decomposing at least one source gas within a thermalizing gas injector to form a group III element precursor; directing the group III element precursor toward a surface of a substrate through at least one gas column to absorb the at least one group III element on a surface of the substrate; directing a group V element precursor toward the surface of the substrate through at least another gas column substantially aligned with the at least one gas column to form a III-V semiconductor material.
The method of Embodiment 12, further comprising establishing movement of the substrate relative to the at least one gas column and the at least another gas column.
The method of Embodiment 13, wherein establishing movement of the substrate relative to the at least one gas column and the at least another gas column comprises establishing movement of the substrate relative to the at least one gas column and the at least another gas column of a plurality of gas columns.
The method of any one of Embodiments 12 through 14, wherein thermally decomposing at least one source gas within a thermalizing injector to form a group III element precursor comprises thermally decomposing least one of GaCl3, InCl3, and AlCl3 within the thermalizing gas injector to form at least one of GaCl, InCl, and AlCl and chlorine gas.
The method of Embodiment 15, further comprising reacting the chlorine gas with at least one of liquid gallium, liquid indium, and liquid aluminum within the thermalizing gas injector to form at least one of additional GaCl, InCl, and AlCl.
The method of Embodiment 15 or Embodiment 16, further comprising reacting the GaCl with at least one of liquid indium, liquid aluminum and liquid iron within the thermalizing gas injector to form at least one of InGaClx, AlGaClx, and FeGaClx.
The method of any one of Embodiments 12 through 17, wherein directing the group III element precursor toward a surface of a substrate through at least one gas column to absorb the at least one group III element on a surface of the substrate comprises directing at least one of GaCl, InCl, and AlCl toward a surface of a substrate through the at least one gas column to absorb at least one of gallium, indium, and aluminum on the surface of the substrate.
The method of Embodiment 18, wherein directing at least one of GaCl, InCl, and AlCl toward a surface of a substrate comprises exposing the substrate to GaCl.
The method of any one of Embodiments 12 through 19, wherein directing a group V element precursor toward the surface of the substrate through at least another gas column comprises directing at least one of nitrogen, arsenic, and phosphorous toward the surface of the substrate through the at least another gas column.
The method of any one of Embodiments 12 through 20, further comprising thermalizing at least one of ammonia, arsine, and phosphine to generate the group V element precursor.
The method of any one of Embodiments 12 through 21, further comprising exposing the surface of the substrate to at least one purge gas to remove at least one of the group III element precursor and the group V element precursor from the surface of the substrate.
A deposition system, comprising: a manifold comprising a plurality of substantially aligned gas columns configured to direct one or more gases, at least one of the substantially aligned gas columns configured to receive a group III precursor gas from a thermalizing gas injector comprising: an inlet; a thermalizing conduit; a liquid container configured to hold a liquid reagent therein; an outlet; and a pathway extending from the inlet, through the thermalizing conduit to an interior space within the liquid container, and from the interior space within the liquid container to the outlet; and at least one assembly for moving a substrate relative to the manifold.
The deposition system of Embodiment 23, wherein the thermalizing conduit has a length greater than a shortest distance between the inlet and the liquid container.
The deposition system of Embodiment 23 or Embodiment 24, further comprising at least one liquid group III element within the liquid container.
The deposition system of Embodiment 25, wherein the at least one liquid group III element comprises at least one of liquid gallium, liquid indium, and liquid aluminum.
The deposition system of any one of Embodiments 23 through 26, wherein at least one of the thermalizing conduit and the liquid container is at least substantially comprised of quartz.
The deposition system of any one of Embodiments 23 through 27, further comprising at least one heating element disposed proximate at least one of the thermalizing conduit and the liquid container.
The deposition system of any one of Embodiments 23 through 27, wherein the at least one heating element comprises a passive heating element at least substantially comprised of at least one of aluminum nitride, silicon carbide, and boron carbide.
The deposition system of any one of Embodiments 23 through 27, further comprising: at least one gas source; and at least one gas inflow conduit configured to carry a source gas from the gas source to the inlet of the thermalizing gas injector.
The deposition system of Embodiment 30, wherein the at least one gas source comprises a source of at least one of GaCl3, InCl3, and AlCl3.
The deposition system of any one of Embodiments 23 through 31, further comprising at least one purge gas nozzle disposed between each of the gas columns of the plurality.
The deposition system of any one of Embodiments 23 through 32, wherein another gas column adjacent the at least one gas column is configured to receive at least one purge gas.
The deposition system of any one of Embodiments 23 through 33, wherein the at least one assembly for moving a substrate relative to the manifold comprises a track system configured to transport the substrate through a series of injection positions along the length of the manifold, each injection position underlying one of the plurality of gas columns.
The embodiments of the invention described above do not limit the scope of the invention, since these embodiments are merely examples of embodiments of the invention, which is defined by the scope of the appended claims and their legal equivalents. Any equivalent embodiments are intended to be within the scope of this invention. Indeed, various modifications of the invention, in addition to those shown and described herein, such as alternate useful combinations of the elements described, will become apparent to those skilled in the art from the description. Such modifications are also intended to fall within the scope of the appended claims.
This application is a continuation of U.S. patent application Ser. No. 13/357,805, filed Jan. 25, 2012, now U.S. Pat. No. 8,486,193, issued Jul. 16, 2013, which application is a divisional of U.S. patent application Ser. No. 12/895,311, filed Sep. 30, 2010, now U.S. Pat. No. 8,133,806, issued Mar. 13, 2012, the disclosure of each of which is incorporated herein in its entirety by this reference. The subject matter of this application is related to the subject matter of U.S. Patent Provisional Application Ser. No. 61/157,112, which was filed on Mar. 3, 2009 in the name of Arena et al., and to the subject matter of U.S. patent application Ser. No. 12/894,724, filed Sep. 30, 2010, now U.S. Pat. No. 8,486,192, issued Jul. 16, 2013, the entire disclosure of each of which is incorporated herein in its entirety by this reference.
| Number | Name | Date | Kind |
|---|---|---|---|
| 3146137 | Williams et al. | Aug 1964 | A |
| 3679949 | Uekusa et al. | Jul 1972 | A |
| 4016589 | Tanimura et al. | Apr 1977 | A |
| 4792467 | Melas | Dec 1988 | A |
| 4839145 | Gale et al. | Jun 1989 | A |
| 5035767 | Nishizawa | Jul 1991 | A |
| 5077875 | Hoke et al. | Jan 1992 | A |
| 5146869 | Bohannon et al. | Sep 1992 | A |
| 5250148 | Nishizawa et al. | Oct 1993 | A |
| 5589110 | Motoda et al. | Dec 1996 | A |
| 5730802 | Ishizumi et al. | Mar 1998 | A |
| 5782980 | Allen et al. | Jul 1998 | A |
| 6080241 | Li et al. | Jun 2000 | A |
| 6090705 | Arena et al. | Jul 2000 | A |
| 6110809 | Sze et al. | Aug 2000 | A |
| 6121140 | Arena et al. | Sep 2000 | A |
| 6126719 | Sturgill et al. | Oct 2000 | A |
| 6153010 | Kiyoku et al. | Nov 2000 | A |
| 6153012 | Rupp et al. | Nov 2000 | A |
| 6179913 | Solomon et al. | Jan 2001 | B1 |
| 6206971 | Umotoy et al. | Mar 2001 | B1 |
| 6207844 | Kouvetakis et al. | Mar 2001 | B1 |
| 6355107 | Solomon et al. | Mar 2002 | B1 |
| 6440494 | Arena-Foster | Aug 2002 | B1 |
| 6495707 | Leese et al. | Dec 2002 | B1 |
| 6569765 | Solomon et al. | May 2003 | B1 |
| 6632725 | Trassoudaine et al. | Oct 2003 | B2 |
| 6689252 | Shamouilian et al. | Feb 2004 | B1 |
| 6733591 | Anderson | May 2004 | B2 |
| 6815362 | Wong et al. | Nov 2004 | B1 |
| 6911083 | Hara | Jun 2005 | B2 |
| 6921062 | Gregg et al. | Jul 2005 | B2 |
| 7011711 | Shreter et al. | Mar 2006 | B2 |
| 7118781 | Sumakeris et al. | Oct 2006 | B1 |
| 7128785 | Kaeppeler et al. | Oct 2006 | B2 |
| 7279047 | Melnik et al. | Oct 2007 | B2 |
| 7413982 | Levy | Aug 2008 | B2 |
| 7456429 | Levy | Nov 2008 | B2 |
| 7501023 | Dmitriev et al. | Mar 2009 | B2 |
| 7572686 | Levy et al. | Aug 2009 | B2 |
| 7608526 | Cody et al. | Oct 2009 | B2 |
| 7670435 | Tsvetkov et al. | Mar 2010 | B2 |
| 8133806 | Werkhoven | Mar 2012 | B1 |
| 20020100418 | Sandhu | Aug 2002 | A1 |
| 20030024475 | Anderson | Feb 2003 | A1 |
| 20030221617 | Lim | Dec 2003 | A1 |
| 20040025370 | Guenther | Feb 2004 | A1 |
| 20050221021 | Strang | Oct 2005 | A1 |
| 20050242061 | Fukuda | Nov 2005 | A1 |
| 20050258459 | Hwang et al. | Nov 2005 | A1 |
| 20060008941 | Haskell et al. | Jan 2006 | A1 |
| 20060011135 | Dmitriev et al. | Jan 2006 | A1 |
| 20060040475 | Emerson | Feb 2006 | A1 |
| 20060042544 | Hasebe et al. | Mar 2006 | A1 |
| 20060115595 | Shenai-Khatkhate et al. | Jun 2006 | A1 |
| 20060226117 | Bertram et al. | Oct 2006 | A1 |
| 20060228473 | Satoh | Oct 2006 | A1 |
| 20060275546 | Arena et al. | Dec 2006 | A1 |
| 20070014990 | Arico et al. | Jan 2007 | A1 |
| 20070190780 | Chung et al. | Aug 2007 | A1 |
| 20070238311 | Levy | Oct 2007 | A1 |
| 20080166880 | Levy | Jul 2008 | A1 |
| 20080166884 | Nelson et al. | Jul 2008 | A1 |
| 20080248200 | Arena et al. | Oct 2008 | A1 |
| 20090081366 | Kerr et al. | Mar 2009 | A1 |
| 20090081842 | Nelson et al. | Mar 2009 | A1 |
| 20090081885 | Levy et al. | Mar 2009 | A1 |
| 20090081886 | Levy et al. | Mar 2009 | A1 |
| 20090130858 | Levy | May 2009 | A1 |
| 20090178611 | Arena et al. | Jul 2009 | A1 |
| 20090205563 | Arena et al. | Aug 2009 | A1 |
| 20090214785 | Arena et al. | Aug 2009 | A1 |
| 20090217878 | Levy et al. | Sep 2009 | A1 |
| 20090223441 | Arena et al. | Sep 2009 | A1 |
| 20090223442 | Arena et al. | Sep 2009 | A1 |
| 20090223453 | Arena et al. | Sep 2009 | A1 |
| 20090283029 | Arena et al. | Nov 2009 | A1 |
| 20100000681 | Bertram et al. | Jan 2010 | A1 |
| 20100041213 | Lee | Feb 2010 | A1 |
| 20100258053 | Arena et al. | Oct 2010 | A1 |
| 20100297846 | Kaga et al. | Nov 2010 | A1 |
| 20120083100 | Bertram, Jr. | Apr 2012 | A1 |
| 20120118233 | Werkhoven | May 2012 | A1 |
| 20130047918 | Bertram, Jr. et al. | Feb 2013 | A1 |
| Number | Date | Country |
|---|---|---|
| 59188118 | Oct 1984 | JP |
| 63045199 | Feb 1988 | JP |
| 63316425 | Dec 1988 | JP |
| 04132681 | May 1992 | JP |
| 07321045 | Dec 1995 | JP |
| 09293681 | Nov 1997 | JP |
| 2005259854 | Sep 2005 | JP |
| 2008066490 | Mar 2008 | JP |
| 0068471 | Nov 2000 | WO |
| 2010024671 | Mar 2010 | WO |
| 2010101715 | Sep 2010 | WO |
| Entry |
|---|
| French Search Report for French Application No. 1058774 dated Jun. 14, 2011, 2 pages. |
| French Written Opinion for French Application No. 1058774 dated Oct. 26, 2010, 5 pages. |
| International Search Report and Written Opinion for International Application No. PCT/US2007/084820 mailed Apr. 9, 2008, 10 pages. |
| International Search Report and Written Opinion for International Application No. PCT/US2007/070721 mailed Feb. 1, 2008, 14 pages. |
| International Search Report and Written Opinion for International Application No. PCT/US2007/084845 dated May 22, 2008, 11 pages. |
| International Search Report and Written Opinion for International Application No. PCT/US2007/084826 mailed Mar. 31, 2008, 7 pages. |
| International Search Report and Written Opinion for International Application No. PCT/US2007/084935 mailed May 7, 2008, 9 pages. |
| Kim et al., Atomic Layer Deposition of GaN Using GaCl3 and NH3, J. Vac. Sci. Technol., Jul./Aug. 2009, vol. A 27, No. 4, pp. 923-928. |
| Lee et al., Vapor Phase Epitaxy of GaN Using AgCl3/N2 and NH3/N2, Journal of Crystal Growth (1996), vol. 169, pp. 689-696. |
| Levy et al., Oxide Electronics by Spatial Atomic Layer Deposition, Journal of Display Technology, Dec. 2009, vol. 5, No. 12, pp. 484-494. |
| Standard Search Report, European Patent Office, dated Jan. 31, 2007. |
| Varadarajan et al., On the Chloride Vapor-Phase Epitaxy Growth of GaN and its Characterization, Journal of Crystal Growth (2004), vol. 260, pp. 43-49. |
| Number | Date | Country | |
|---|---|---|---|
| 20130295708 A1 | Nov 2013 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 12895311 | Sep 2010 | US |
| Child | 13357805 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 13357805 | Jan 2012 | US |
| Child | 13933855 | US |