The present disclosure relates to the processing of substrates. In particular, it provides a novel method and process flow for forming a passivation layer on sidewall surfaces of an amorphous carbon layer (ACL) to avoid bowing during an ACL etch process.
As geometries in substrate processing continue to shrink, the technical challenges to forming structures on substrates via photolithography and etch techniques increase. As requirements for smaller geometry structures arose, a variety of techniques have been utilized for achieving suitable structures. Although reduced feature sizes are achieved, pattern performance problems have occurred in some conventional small geometry patterning and etch methods.
For example, photolithography techniques have been used to transfer patterns from a patterned layer to an organic mask layer, such as an amorphous carbon layer (ACL) film, underlying the patterned layer. ACL films are often used as a hard mask for patterning underlying layers using a variety of small geometry patterning methods. However, as feature sizes decrease, critical dimensions (“CDs”) become smaller and aspect ratios increase, leading to increasingly greater etch depths. Accordingly, high ion energy is often required to etch high-aspect ratio features (such as vias, contact holes and lines) in ACL films and underlying layers. When etching high-aspect ratio features, the thickness of the ACL film may be increased to withstand etching of the underlying layers. Increasing the thickness of the ACL, however, can create defects in the etched features.
For example, “bowing” may occur when conventional pattern transfer techniques are used to etch high-aspect ratio features in ACL films. Bowing occurs when plasma ions bombard sidewall surfaces of the ACL film to laterally etch the sidewall surfaces. The “bow CD” is measurement of bowing, which is generally defined as the cross-section or width of an opening formed in a layer in a direction perpendicular to the thickness of the layer. When bowing occurs, the bow CD is typically larger near the top of the layer than the bottom of the layer.
In conventional pattern transfer processes, the patterned substrate 100 is exposed to light during a lithography step, and a wet or dry etch process is performed after the lithography step to remove the exposed portions of the hard mask layer 106 to create openings 110. When a dry process is used, a process gas is converted by high-energy power into plasma and ions, which bombard exposed portions of the hard mask layer 106. Although ion bombard is primarily anisotropic, ion scattering caused by collision of molecules in the plasma may lead to lateral etching of the opening 110 sidewalls and bowing. As shown in
In
As known in the art, atomic layer deposition (ALD) is a process wherein conventional chemical vapor deposition (CVD) processes are divided into separate deposition steps to construct a thin film by sequentially depositing single atomic monolayers in each deposition step. The ALD technique is based on the principle of the formation of a saturated monolayer of reactive precursor molecules by chemisorption. A typical ALD process consists of injecting a first precursor for a period of time until a saturated monolayer is formed on the substrate. Then, the first precursor is purged from the chamber using an inert gas to prevent the first precursor from mixing with a subsequent precursor gas species. After the chamber is purged, a second precursor is injected into the chamber, also for a period of time, thus forming a layer on the substrate from the reaction of the second precursor with the monolayer formed on the substrate. Then, the second precursor is purged from the chamber and the process of introducing the first precursor, purging the process chamber, introducing the second precursor, and purging the process chamber is often repeated a number of times to achieve a desired film thickness.
A wide range of ALD processes have been used to form ALD passivation layers on sidewall surfaces of hard mask layers. For example, ALD processes have been used to form silicon dioxide (SiO2) passivation layers on the sidewall surfaces of hard mask layers by utilizing a cyclical process of exposing the substrate to a silicon precursor gas (e.g., silanes) followed by exposure to an oxygen-containing gas (e.g., oxygen, O2, ozone, O3, etc.). Other ALD processes have been used to form silicon nitride (SiN) passivation layers on the sidewall surfaces of hard mask layers by exposing the substrate to a silicon precursor gas (e.g., silanes) followed by exposure to an nitrogen-containing gas (e.g., nitrogen, N2, ammonia, NH3, etc.) in a cyclical process. In either case, the cyclical process of introducing a silicon precursor gas, purging the chamber, introducing the oxygen- or nitrogen-containing gas and purging the chamber is time consuming. Thus, throughput is reduced when ALD processes are used to form passivation layers on the sidewall surfaces of hard mask layers. Further, the ALD processes may contribute to sidewall roughness which may negatively impact the performance of the formed structures such as vias or contact holes.
As such, a need exists for an improved process and method for forming a passivation layer on sidewall surfaces of an amorphous carbon layer (ACL) to avoid bowing during an ACL etch process.
Improved process flows and methods are provided herein for forming a passivation layer on sidewall surfaces of openings formed in an amorphous carbon layer (ACL) to avoid bowing during an ACL etch process. More specifically, improved process flows and methods are provided to form a silicon-containing passivation layer on sidewall surfaces of the openings created within the ACL without utilizing atomic layer deposition (ALD) techniques or converting the silicon-containing passivation layer to an oxide or a nitride. As such, the improved process flows and methods disclosed herein may be used to protect the sidewall surfaces of the ACL and prevent bowing during the ACL etch process, while also reducing processing time and improving throughput.
In one embodiment, a method for patterning a substrate is provided. The method may comprise forming an amorphous carbon layer (ACL) on one or more underlying layers formed on the substrate, wherein a thickness of the ACL is greater than 1 micrometer (μm) and forming a patterned layer over the ACL. The method further comprises etching exposed portions of the ACL not covered by the patterned layer to create openings in the ACL, wherein the exposed portions of the ACL are partially etched to a first depth, which is less than the thickness of the ACL. The method further comprises forming a silicon-containing passivation layer on sidewall surfaces of the openings created in the ACL by exposing the substrate to a silicon-containing precursor. The method then comprises continuing etching the exposed portions of the ACL to a second depth, which is greater than the first depth, without converting the silicon-containing passivation layer to an oxide or a nitride.
Variations of the method described above may be performed wherein said forming the silicon-containing passivation layer comprises exposing the substrate to the silicon-containing precursor in an absence of plasma to deposit a silicon monolayer on the sidewall surfaces of the openings created in the ACL. In another variation, said forming the silicon-containing passivation layer further comprises: (1) subsequently exposing the substrate to a hydrogen plasma to change a surface property of the silicon monolayer; and (2) repeating said exposing the substrate to the silicon-containing precursor in the absence of plasma and said subsequently exposing the substrate to the hydrogen plasma a number of times to form a plurality of silicon monolayers on the sidewall surfaces of the openings. In another variation, an atomic layer deposition (ALD) process is not used to deposit the silicon monolayer.
In yet another variation, said exposing the substrate to the silicon-containing precursor in the absence of plasma comprises: (1) providing the substrate within a plasma chamber coupled to a first radio frequency (RF) source and a second RF source; and (2) supplying the silicon-containing precursor to the plasma chamber without supplying power from the first RF source or the second RF to the plasma chamber. In still another embodiment, said providing the substrate within the plasma chamber comprises providing the substrate within a capacitively coupled plasma (CCP) chamber or an inductively coupled plasma (ICP) chamber.
In another embodiment, the silicon-containing precursor comprises an aminosilane. In yet another embodiment, the silicon-containing precursor comprises di-isopropylaminosilane. In some embodiments, the method further comprises repeating said forming the silicon-containing passivation layer on sidewall surfaces of the openings and said continuing etching the exposed portions of the ACL a number of cycles and/or until the exposed portions of the ACL are completely removed. In some embodiments, the number of cycles is 5 or more.
In a second embodiment, a method for patterning a substrate is provided. The method comprises: forming an amorphous carbon layer (ACL) on one or more underlying layers formed on the substrate, wherein a thickness of the ACL is greater than 1 micrometer (μm); forming a patterned mask layer over the ACL; and etching exposed portions of the ACL not covered by the patterned mask layer to create openings in the ACL, wherein the exposed portions of the ACL are partially etched to a first depth, which is less than the thickness of the ACL. The method further comprises exposing the substrate to a silicon-containing precursor in an absence of plasma to form a silicon monolayer on sidewall surfaces of the openings created in the ACL, and subsequently exposing the substrate to a hydrogen plasma to change a surface property of the silicon monolayer. The method also comprises forming a plurality of silicon monolayers on the sidewall surfaces of the openings by repeating said exposing the substrate to the silicon-containing precursor in the absence of plasma and said subsequently exposing the substrate to the hydrogen plasma a number of times. The method also comprise continuing etching the exposed portions of the ACL to a second depth, which is greater than the first depth.
The second embodiment may further comprise repeating said forming the plurality of silicon monolayers on the sidewall surfaces of the openings and said continuing etching the exposed portions of the ACL a number of cycles and/or until the exposed portions of the ACL are completely removed. In alternative, an atomic layer deposition (ALD) process is not used to form the silicon monolayer or the plurality of silicon monolayers. The second embodiment may further include said exposing the substrate to the silicon-containing precursor in the absence of plasma comprising: (1): providing the substrate within a plasma chamber coupled to a first radio frequency (RF) source and a second RF source; and (2) supplying the silicon-containing precursor to the plasma chamber without supplying power from the first RF source or the second RF to the plasma chamber. In another variation, said providing the substrate within the plasma chamber comprises providing the substrate within a capacitively coupled plasma (CCP) chamber or an inductively coupled plasma (ICP) chamber. In some variations, the silicon-containing precursor comprises an aminosilane. In some variations the silicon-containing precursor comprises di-isopropylaminosilane. In some variations, the plurality of silicon monolayers are not converted to an oxide or a nitride. In some variations, the number of times is three or more.
A more complete understanding of the present inventions and advantages thereof may be acquired by referring to the following description taken in conjunction with the accompanying drawings, in which like reference numbers indicate like features. It is to be noted, however, that the accompanying drawings illustrate only exemplary embodiments of the disclosed concepts and are therefore not to be considered limiting of the scope, for the disclosed concepts may admit to other equally effective embodiments.
Improved process flows and methods are provided herein for forming a passivation layer on sidewall surfaces of openings formed in an amorphous carbon layer (ACL) to avoid bowing during an ACL etch process. More specifically, improved process flows and methods are provided to form a silicon-containing passivation layer on sidewall surfaces of the openings created within the ACL without utilizing atomic layer deposition (ALD) techniques or converting the silicon-containing passivation layer to an oxide or a nitride. As such, the improved process flows and methods disclosed herein may be used to protect the sidewall surfaces of the ACL and prevent bowing during the ACL etch process, while also reducing processing time and improving throughput.
In the present disclosure, a patterned substrate is provided with an amorphous carbon layer (ACL), which is formed on one or more underlying layers, and a patterned layer formed over the ACL. In some embodiments, a thickness of the ACL may be greater than 1 micrometer (μm). After partially etching exposed portions of the ACL to a first depth to create openings within the ACL, the improved process flows and methods disclosed herein form a silicon-containing passivation layer on sidewall surfaces of the openings by exposing the patterned substrate to a silicon-containing precursor gas. In some embodiments, the silicon-containing precursor gas may comprise an aminosilane precursor, such as but not limited to, di-isopropylaminosilane (SiH3N(C3H7)2, otherwise referred to as LTO520). Other aminosilane and silicon-containing precursor gases may also be used. For example, other precursors may include, but are not limited to, tetraethoxysilane (TEOS), tetramethoxysilane (TMOS), dichlorosilane (DCS), tetrachlorosilane (SiCl4), etc.
In a first embodiment, the silicon-containing passivation layer may be formed by exposing the patterned substrate to the silicon-containing precursor gas in the absence of plasma to deposit a silicon monolayer on the sidewall surfaces of the openings created in the ACL. This may be achieved, in some embodiments, by providing the patterned substrate within a plasma chamber coupled to a first radio frequency (RF) source and a second RF source, and supplying the silicon-containing precursor to the plasma chamber without supplying power from the first RF source or the second RF to the plasma chamber. In some embodiments, the plasma chamber may be a capacitively coupled plasma (CCP) chamber or an inductively coupled plasma (ICP) chamber. However, such chambers are exemplary and other deposition chambers and techniques, including non-plasma chambers may be utilized.
In a second embodiment, the silicon-containing passivation layer may be formed by: (a) exposing the patterned substrate to the silicon-containing precursor gas in the absence of plasma to form a silicon monolayer on the sidewall surfaces of the openings created in the ACL, (b) subsequently exposing the substrate to a hydrogen plasma to change a surface property of the silicon monolayer, and (c) repeating the steps of exposing the substrate to the silicon-containing precursor in the absence of plasma and subsequently exposing the substrate to a hydrogen plasma a number of times to form a plurality of silicon monolayers on the sidewall surfaces of the openings.
After the silicon-containing passivation layer is formed, the improved process flows and methods disclosed herein continue etching the exposed portions of the ACL to a second depth, which is greater than the first depth. If the second depth is less than the thickness of the ACL, the improved process flows and methods disclosed herein may repeat the process of forming silicon-containing passivation layer(s) on the sidewall surfaces of the openings and continue etching the exposed portions of the ACL for a number of cycles and/or until the exposed portions of the ACL are completely removed.
Unlike conventional processes, the silicon-containing passivation layer described herein is formed without utilizing atomic layer deposition (ALD) techniques or converting the silicon-containing passivation layer to an oxide or a nitride. Thus, the disclosed process flows and methods protect the sidewall surfaces of the ACL and prevent bowing during the ACL etch process, while reducing processing time and improving throughput. In the first embodiment, better clogging margin may be achieved by using a thinner passivation layer (i.e., a silicon monolayer). However, better sidewall protection may be achieved in the second embodiment by alternating between non-plasma and plasma processes to build the silicon monolayers up to provide a substantially thicker passivation layer.
As shown in
Base substrate 302 may be any substrate for which the use of patterned features is desirable. For example, base substrate 302 may be a semiconductor substrate having one or more semiconductor processing layers formed thereon. In one embodiment, base substrate 302 may be a substrate that has been subject to multiple semiconductor processing steps which yield a wide variety of structures and layers, all of which are known in the substrate processing art.
Oxide layer 304 may be formed from any of a wide variety of materials, as is known in the art. In one embodiment, the oxide layer 304 may be any of a variety of oxide containing layers, such as but not limited to, a silicon dioxide (SiO2) layer, a multi-layered oxide-nitride-oxide-nitride (ONON), a multi-layered oxide-polysilicon-oxide-polysilicon (OPOP), or layers containing an oxide. Oxide layer 304 may be formed using any of a wide variety of deposition processes as is well known in the art, such as but not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD), capacitively coupled plasma (CCP) deposition, inductively coupled plasma (ICP) deposition, spin-on processes, atomic layer deposition (ALD), etc. In one embodiment, a silicon containing oxide layer is formed using TEOS chemical vapor deposition techniques. In some embodiments, one or more layers may be formed above and/or below the oxide layer 304 shown in
ACL 306 may also be formed from any of a wide variety of materials using any of a wide variety of deposition processes, as is known in the art. Examples of deposition processes that may be used to form ACL 306 include, but are not limited to, chemical vapor deposition (e.g., CVD, PECVD), physical vapor deposition (PVD), plasma deposition (e.g., CCP, ICP), spin-on processes, etc. In one or more of the deposition processes described above, ACL 306 may be deposited by exposing the patterned substrate 100 to a gas mixture comprising a hydrocarbon gas (e.g., CxHy) and an inert gas (e.g., N2, Ar, He, Ne, Kr, Xe, etc.), possibly in combination with other gas sources, such as for example, a hydrogen-containing gas (e.g., H2), a nitrogen-containing gas (e.g., N2, NH3), etc.
In some embodiments, ACL 306 is used as a hard mask layer for etching high-aspect ratio features (such as vias, contact holes and lines) in one or more of the underlying layers. When etching high-aspect ratio features, the thickness of the ACL 306 may be increased to withstand etching of the ACL 306 and the one or more underlying layers. In some embodiments, the thickness (T) of the ACL 306 may be greater than 1 μm (micrometer). For example, the thickness of the ACL 306 may range between 1 μm and 4 μm. Further, feature widths and spaces of 300 nm or smaller and even 70 nm or smaller may be necessary to be formed in the ACL 306. Thus, high aspect ratio features may need to be formed in the ACL 306. Thus, aspect ratios of 10, 50 or even higher may be formed.
After ACL 306 is formed, a patterned layer 308 may be formed on the ACL 306 by depositing one or more material layers onto the ACL 306 and then patterning the material layer(s) using a lithography technique. A variety of deposition processes and a variety of lithography techniques may be used to form the patterned layer 308, as is well known in the art. In addition, the patterned layer 308 may generally be formed from any of a wide variety of mask materials commonly used in lithography. For example, the patterned layer 308 may comprise a photoresist layer or other mask layers (for instance a mask layer that was patterned from a photoresist lithography and etch process as is known in the art), etc.
After the patterned layer 308 is formed, an ACL etch process 312 may be performed to remove exposed portions of the ACL 306 (i.e., portions of the ACL 306 not protected by the patterned layer 308) to create openings 310 in the ACL 306. As shown in
Various etch chemistries may be used in the ACL etch process 312 shown in
In one example embodiment, the ACL etch process 312 shown in
As noted above, the ACL etch process 312 shown in
After partially etching the exposed portions of the ACL 306 to create openings 310 in
Silicon-containing passivation layer 316 may be formed using any of a wide variety of deposition processes, such as but not limited to, chemical vapor deposition (e.g., CVD, PECVD), physical vapor deposition (PVD), and plasma deposition (e.g., CCP, ICP) processes. The silicon-containing passivation layer 316, however, does not need to be formed as part of an atomic layer deposition (ALD) process. As noted above, ALD processes build up monolayers on a substrate surface by alternately exposing the substrate to a first precursor and a second precursor, while purging the processing chamber in between precursor gas exposure to prevent the first and second precursors from mixing. For example, conventional ALD processes have been used to form silicon dioxide (SiO2) or silicon nitride (SiN) passivation layers on sidewall surfaces of hard mask layers by alternately exposing the substrate to a silicon precursor gas (e.g., silanes) followed by exposure to an oxygen-containing gas (e.g., O2, O3, etc.) or a nitrogen-containing gas (e.g., N2, NH3, etc.). These ALD processes are time consuming and limit throughput.
In one embodiment, the silicon-containing passivation layer 316 shown in
In one example embodiment, the silicon-containing passivation layer 316 may be formed on sidewall surfaces of the openings 310 by supplying a gas mixture comprising approximately 50 to 150 sccm of LTO520 and approximately 50 to 150 sccm of argon (Ar) to a plasma chamber (e.g., a CCP or ICP chamber) in which the patterned substrate 100 is disposed. Other gas mixtures may also be used. The gas mixture may be supplied to the plasma chamber at zero source power (0 W), zero bias power (0 W), relatively high chamber pressure (e.g., 200 to 400 mT) and relatively high temperature (e.g., 30 to 100° C.). Other process conditions may also be used.
In some embodiments, the ACL etch process 312 may continue after the silicon monolayer is formed in
In other embodiments, the processing steps shown in
In other embodiments, the silicon-containing passivation layer 316 may be formed by: (a) exposing the patterned substrate 100 to the silicon-containing precursor 314 in the absence of plasma to deposit a silicon monolayer on the sidewall surfaces of the openings 310, as shown in
In one example embodiment, the hydrogen plasma 315 may be generated by supplying approximately 100 to 300 sccm of hydrogen (H2) to a plasma chamber (e.g., a CCP or ICP chamber) in which the patterned substrate 100 is disposed. Other hydrogen containing gases may also be used. The hydrogen containing gas may be supplied to the plasma chamber at relatively high source power (e.g., 300 to 700 W), little to no bias power (e.g., 0 W), relatively low chamber pressure (e.g., 30 to 70 mT) and relatively high temperature (e.g., 50 to 100° C.). High chamber pressures (e.g. 100 to 500 mT) may also be utilized. Other process conditions may also be used. Other hydrogen-containing gases, such as for example, ammonia (NH3) may be utilized and inert gases (such as Ar, N2, He, Ne, Kr, Xe) may alternatively be used or added to the gas flow. N2 plasma processes may also be utilized.
Exposing the patterned substrate 100 to the hydrogen plasma 315 allows the thickness of passivation layer 316 to increase. The increase may result from various mechanisms, such as for example, but not limited to, surface property changes that allow the buildup of additional silicon monolayers, more complete silicon coverage due to making unabsorbed sites more active, etc. This results in the formation of a substantially thicker passivation layer 316, which provides better sidewall protection when the ACL etch process 312 resumes than can be provided with a single silicon monolayer. However, exposure to the hydrogen plasma 315 does not convert the silicon monolayer to another material, such as an oxide or nitride. This enables improved throughput as opposed to ALD techniques.
In some embodiments, the ACL etch process 312 may continue in
In other embodiments, the processing steps shown in
Further, the method 400 may include forming a silicon-containing passivation layer on sidewall surfaces of the openings created in the ACL by exposing the substrate to a silicon-containing precursor (in step 440). For example, the silicon-containing passivation layer may be formed (in step 440) by exposing the substrate to the silicon-containing precursor in the absence of plasma to deposit a silicon monolayer on the sidewall surfaces of the openings created in the ACL. After the silicon monolayer is deposited on the sidewall surfaces of the openings, the method 400 may continue etching the exposed portions of the ACL to a second depth, which is greater than the first depth, without converting the silicon-containing passivation layer to an oxide or a nitride (in step 450). In some embodiments, method 400 may repeat said forming a silicon-containing passivation layer on sidewall surfaces of the openings (in step 440) and said continuing etching the exposed portions of the ACL (in step 450) for a number of cycles and/or until the exposed portions of the ACL are completely removed.
The method 500 may further include exposing the substrate to a silicon-containing precursor in the absence of plasma to form a silicon monolayer on sidewall surfaces of the openings created in the ACL (in step 540), subsequently exposing the substrate to a hydrogen plasma to change a surface property of the silicon monolayer (in step 550), and forming a plurality of silicon monolayers on the sidewall surfaces of the openings by repeating said exposing the substrate to the silicon-containing precursor in the absence of plasma and said subsequently exposing the substrate to a hydrogen plasma a number of times (in step 560). After the plurality of silicon monolayers are formed on the sidewall surfaces of the openings, the method 500 may continue etching the exposed portions of the ACL to a second depth, which is greater than the first depth (in step 570). In some embodiments, method 500 may repeat said forming a plurality of silicon monolayers on the sidewall surfaces of the openings (in step 560) and said continuing etching the exposed portions of the ACL (in step 570) for a number of cycles and/or until the exposed portions of the ACL are completely removed.
The process flow shown in
The plasma processing system 700 can be used for a wide variety of operations including, but not limited to, etching, deposition, cleaning, plasma polymerization, plasma-enhanced chemical vapor deposition (PECVD), and so forth. The structure of a plasma processing system 700 is well known, and the particular structure provided herein is merely of illustrative purposes. It will be recognized that different and/or additional plasma process systems may be implemented while still taking advantage of the techniques described herein.
Looking in more detail to
Components of the plasma processing system 700 can be connected to, and controlled by, a control unit 770 that in turn can be connected to a corresponding memory storage unit and user interface (all not shown). Various plasma processing operations can be executed via the user interface, and various plasma processing recipes and operations can be stored in a storage unit. Accordingly, a given substrate can be processed within the plasma processing chamber 705 with various microfabrication techniques. It will be recognized that control unit 770 may be coupled to various components of the plasma processing system 700 to receive inputs from and provide outputs to the components.
The control unit 770 can be implemented in a wide variety of manners. For example, the control unit 770 may be a computer. In another example, the control unit 770 may include one or more programmable integrated circuits that are programmed to provide the functionality described herein. For example, one or more processors (e.g., microprocessor, microcontroller, central processing unit, etc.), programmable logic devices (e.g., complex programmable logic device (CPLD)), field programmable gate array (FPGA), etc.), and/or other programmable integrated circuits can be programmed with software or other programming instructions to implement the functionality of a proscribed process recipe. It is further noted that the software or other programming instructions can be stored in one or more non-transitory computer-readable mediums (e.g., memory storage devices, FLASH memory, dynamic random access (DRAM) memory, reprogrammable storage devices, hard drives, floppy disks, DVDs, CD-ROMs, etc.), and the software or other programming instructions when executed by the programmable integrated circuits cause the programmable integrated circuits to perform the processes, functions, and/or capabilities described herein. Other variations could also be implemented.
During some processing steps, the plasma processing system 700 may apply power from the first RF source 730 and the second RF source 740 to the upper and lower electrodes to generate a plasma 760 in the process chamber 705. When a plasma 760 is generated within the process chamber 705, ions within the plasma 760 are attracted to the substrate 710. The generated plasma 760 can be used for processing a target substrate (such as substrate 710 or any material to be processed) in various types of treatments such as, but not limited to, plasma etching, deposition and/or sputtering. For example, plasma 760 may be generated within the process chamber 705 to perform one or more of the process steps shown in
In the CCP processing system shown in
In one example plasma processing system, for example, the first RF source 730 may provide about 0 to 1400 W of source power in a high-frequency (HF) range from about 3 MHz to 150 MHz (or above) to the upper electrode 720, and the second RF source 740 may provide about 0 to 1400 W of bias power in a low-frequency (LF) range from about 0.2 MHz to 60 MHz to the lower electrode 725. Different operational ranges can also be used depending on type of plasma processing system and the type of treatments (e.g., etching, deposition, sputtering, etc.) performed therein.
In one exemplary embodiment, the ACL etch process 312 shown in
In one exemplary embodiment, the deposition step shown in
In one exemplary embodiment, the plasma step shown in
It is noted that the techniques described herein may be utilized within a wide range of plasma processing systems. Although a particular plasma processing system 700 is shown in
It is noted that various deposition and etch processes can be used to form one or more of the material layers shown and described herein. For example, one or more depositions can be implemented using chemical vapor deposition (e.g., CVD, PECVD), physical vapor deposition (PVD), plasma deposition (e.g., CCP, ICP), spin-on processes, atomic layer deposition (ALD), and/or other deposition processes. In one example deposition process, a gas mixture including but not limited to LTO520, is utilized. However, other aminosilanes and/or silicon-containing precursor gases may also be used. The process may optionally include a combination with one or more dilution gases (e.g., argon, nitrogen, etc.). The process may occur at a variety of pressure, power, flow, and temperature conditions to form a silicon-containing passivation layer on sidewall surfaces of openings formed in an amorphous carbon layer.
It is further noted that various etch processes can be used to etch one or more of the material layers shown and described herein. For example, one or more etch processes can be implemented using plasma etch processes, discharge etch processes, and/or other desired etch processes. In one example plasma etch process, a gas mixture including but not limited to SO2 and O2 optionally in combination with one or more dilution gases (e.g., argon, nitrogen, etc.) can be used at a variety of pressure, power, flow and temperature conditions to etch the exposed portions of the amorphous carbon layer.
Other operating variables for process steps can also be adjusted to control the various deposition and/or etch processes described herein. The operating variables may include, for example, the chamber temperature, chamber pressure, flowrates of gases, types of gases, and/or other operating variables for the processing steps. Variations can also be implemented while still taking advantage of the techniques described herein.
It is noted that reference throughout this specification to “one embodiment” or “an embodiment” means that a particular feature, structure, material, or characteristic described in connection with the embodiment is included in at least one embodiment of the invention, but do not denote that they are present in every embodiment. Thus, the appearances of the phrases “in one embodiment” or “in an embodiment” in various places throughout this specification are not necessarily referring to the same embodiment of the invention. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments. Various additional layers and/or structures may be included and/or described features may be omitted in other embodiments.
The term “substrate” as used herein means and includes a base material or construction upon which materials are formed. It will be appreciated that the substrate may include a single material, a plurality of layers of different materials, a layer or layers having regions of different materials or different structures in them, etc. These materials may include semiconductors, insulators, conductors, or combinations thereof. For example, the substrate may be a semiconductor substrate, a base semiconductor layer on a supporting structure, a metal electrode or a semiconductor substrate having one or more layers, structures or regions formed thereon. The substrate may be a conventional silicon substrate or other bulk substrate comprising a layer of semi-conductive material. As used herein, the term “bulk substrate” means and includes not only silicon wafers, but also silicon-on-insulator (“SOI”) substrates, such as silicon-on-sapphire (“SOS”) substrates and silicon-on-glass (“SOG”) substrates, epitaxial layers of silicon on a base semiconductor foundation, and other semiconductor or optoelectronic materials, such as silicon-germanium, germanium, gallium arsenide, gallium nitride, and indium phosphide. The substrate may be doped or undoped.
Systems and methods for processing a substrate are described in various embodiments. The substrate may include any material portion or structure of a device, particularly a semiconductor or other electronics device, and may, for example, be a base substrate structure, such as a semiconductor substrate or a layer on or overlying a base substrate structure such as a thin film. Thus, the term “substrate” is not intended to be limited to any particular base structure, underlying layer or overlying layer, patterned or unpatterned, but rather, is contemplated to include any such layer or base structure, and any combination of layers and/or base structures.
One skilled in the relevant art will recognize that the various embodiments may be practiced without one or more of the specific details, or with other replacement and/or additional methods, materials, or components. In other instances, well-known structures, materials, or operations are not shown or described in detail to avoid obscuring aspects of various embodiments of the invention. Similarly, for purposes of explanation, specific numbers, materials, and configurations are set forth in order to provide a thorough understanding of the invention. Nevertheless, the invention may be practiced without specific details. Furthermore, it is understood that the various embodiments shown in the figures are illustrative representations and are not necessarily drawn to scale.
Further modifications and alternative embodiments of the described systems and methods will be apparent to those skilled in the art in view of this description. It will be recognized, therefore, that the described systems and methods are not limited by these example arrangements. It is to be understood that the forms of the systems and methods herein shown and described are to be taken as example embodiments. Various changes may be made in the implementations. Thus, although the inventions are described herein with reference to specific embodiments, various modifications and changes can be made without departing from the scope of the present inventions. Accordingly, the specification and figures are to be regarded in an illustrative rather than a restrictive sense, and such modifications are intended to be included within the scope of the present inventions. Further, any benefits, advantages, or solutions to problems that are described herein with regard to specific embodiments are not intended to be construed as a critical, required, or essential feature or element of any or all the claims.
Number | Name | Date | Kind |
---|---|---|---|
20180130669 | Lane | May 2018 | A1 |