Any and all applications for which a foreign or domestic priority claim is identified in the Application Data Sheet as filed with the present application are hereby incorporated by reference under 37 CFR 1.57.
The present invention is the result of a joint research agreement between ASM International, N.V. and Technische Universiteit Endhoven (Eindhoven University of Technology).
The present invention relates generally to atomic layer deposition (ALD), and more particularly to identification and use of optimal conditions during plasma phases.
In recent years atomic layer deposition (ALD) has been adopted as a manufacturing technique in several fields, including the semiconductor industry. ALD deposits films in a cyclical process, typically alternating exposure of the substrate to two or more reactants in phases separated in time and/or space, where each phase has a self-limiting effect. For example, one phase of the cycle can chemically adsorb, in a self-limiting fashion, a monolayer or less of a precursor or fragment thereof in each cycle. Often the adsorption is self-limited due to ligands of the precursor being inert relative to the adsorbed species, such that after the substrate surface is saturated the adsorption process stops. Reactants in a subsequent phase can react with the adsorbed species to remove the condition that limits the adsorption, such as stripping away ligands form the adsorbed species, for example by chemical reduction or replacement reactions, such that the precursor can again adsorb in a self-limiting fashion in a subsequent cycle. In one example, less than a monolayer of an organic silicon precursor can adsorb in a first phase, and an oxygen-containing reactant can strip the organic ligands from the adsorbed species and leave oxygen in a second phase.
More complicated ALD recipes may include three, four or more reactants, and relative frequencies of the phases may be adjusted to tune the composition of the layer being formed. Typically, each cycle leaves about a molecular monolayer or less per cycle. Many ALD processes average one monolayer every 3-10 cycles because of variety of reasons, such as steric hindrance from large precursor molecules prevents access to all reaction sites in a single cycle, lack or low number of reactive sites or other reasons. Mutually reactive reactants can be kept separated in time and/or space, e.g., by separating pulses by purging, or moving the substrate through different zones with separate reactants. However, variations on the process, such as schemes providing hybrid ALD and chemical vapor deposition (CVD) reactions, can obtain more than a monolayer per cycle.
Despite rather slow growth rates compared to traditional deposition techniques, such as sputter deposition and CVD, ALD has been growing in popularity for several reasons. For example, in the semiconductor industry, ALD can provide much greater step coverage, or conformal growth, or smoother or more uniform films over complex topography compared to other deposition techniques, particularly for very thin layers over structures with high aspect ratios. Need for such conformal layers tends to increase as circuits become more dense. Because the technique is self-limiting in each cycle, and because usually the growth rate tends to be independent of small temperature variations over a substrate, ALD offers almost perfect step coverage. Moreover, ALD tends to involve lower temperatures than other deposition techniques, which also becomes more important with successive generations of integrated circuits in order to conserve ever-stricter thermal budgets and preserve precise device junction depths. Similarly, ALD is increasingly attractive to other industries that could benefit from ultrathin, conformal and/or low temperature depositions.
To preserve self-limiting nature of ALD it can be important to prevent thermal breakdown of precursors that are meant to adsorb largely intact. Thermal breakdown can lead to time-dependent CVD growth mechanisms which can nullify the conformal deposition advantages of ALD. At the same time, some precursors demand significant energy to react with adsorbed species. Ensuring these competing conditions are satisfied can involve delicate trade-offs between substrate temperatures and prolonged exposures to ensure saturative surface reactions.
Plasma ALD processes, sometimes referred to as plasma assisted ALD or plasma enhanced ALD (PEALD), have been developed in order to improve the reaction energy of some phases without increasing the temperature of the substrate. For example, an organic or halide reactant can adsorb less than a monolayer in a first phase, and a second phase can expose the substrate to the products of a nitrogen-, hydrogen- or oxygen-containing plasma to strip ligands from the adsorbed species and/or leave nitrogen or oxygen in the film. However, in some cases it has been difficult to obtain high quality films using conventional plasma ALD techniques.
In one aspect, a method is provided for depositing a layer of silicon nitride by plasma atomic layer deposition. The method includes providing a substrate in a reaction space. In a first phase, the substrate is contacted with a silicon precursor to adsorb an adsorbed species of the silicon precursor on the substrate. In a second phase, the substrate is contacted with excited nitrogen species to react with the adsorbed species. The excited nitrogen species is supplied to or formed in the reaction space for greater than about 0.1 s, and a residence time of the gas species during second phase in the reaction space is less than about 1.0 s.
In another aspect, a method is provided for tuning a plasma atomic layer deposition (ALD) process. The method includes conducting a plasma ALD process to deposit a layer. The plasma ALD process has an adsorption phase and a plasma phase. A quality of the layer is measured. A residence time for the plasma phase is modulated to form a modified version of the plasma ALD process. The modified version of the ALD process is conducted to deposit a further layer, and the quality of the further layer is measured.
In another aspect, a method of optimizing a plasma ALD process is provided. The method includes optimizing impurity levels in films deposited by the plasma ALD process by modulating residence time for excited species in a reaction space volume.
As noted in the Background section above, despite the theoretical advantages that plasma ALD provide in lowering substrate temperatures, thereby preserving thermal budgets and opening the door to precursors that might decompose at higher temperatures, it has been difficult to obtain high quality films, particularly dielectric films such as silicon oxides, metal oxides and silicon nitrides.
Somewhat counterintuitively, the inventors have found that in plasma ALD of certain materials, limiting the gases' residence time in the reaction space for each plasma phase can improve the quality of the film, indicating a fuller reaction can be achieved with lower exposure time to the excited species. Herein reference is made to excited species' or plasma products' residence time for convenience. It will be understood, however, that the residence time applies to all vapor phase species supplied through the reaction space during the plasma phase, including any non-excited species. Conventionally, ALD designers have tended to prolong reactant exposure times to achieve saturation of surface reactions, or modulated other parameters, such as temperature, pressure or plasma power, in attempts to optimize deposition speed and quality. Moreover, a prolonged exposure to reactants would be expected to lead to more efficient saturation with the least amount of reactant. However, conventional attempts at optimization have not been satisfactory for many plasma ALD processes, particularly for dielectric oxides and nitrides. For example, depositing silicon nitride from alternation of organic precursors with nitrogen plasma products has been found to produce poor film density, wet etch rates and/or impurity levels. According to the teachings herein, reducing plasma reactant residence time can increase film quality, and modulating residence time against measured film quality can improve film quality (e.g., low impurity levels, high density).
For convenience of description, the reactant that is adsorbed in the plasma ALD process is referred to herein as a precursor, while the excited species is referred to as a reactant. It will be understood that both the precursor and the excited species serve as ALD reactants, and also that the excited species can also serve as a precursor to the extent it leaves elements in the deposited film. In dielectric film deposition examples, excited nitrogen or excited oxygen species can perform exchange reactions with ligands from a prior adsorbed layer. Also for convenience, the substrate is considered to include previously deposited or adsorbed materials, such that references to contacting the substrate will be understood to include contacting previously deposited or adsorbed materials.
In the first illustrated block 10, the first reactant, or precursor, contacts a substrate to adsorb thereon. It will be understood that the adsorbed species may comprise a fragment of the precursor molecule, such that some ligands may be lost in the process, but that the precursor is not thermally decomposed. In the next block 20, any excess precursor is removed from the reaction space Typically supply of the precursor is stopped at this stage. Such removal can be accomplished, e.g., by purging the reaction chamber or space, pump down, moving the substrate away from a zone in which the precursor is supplied, or combinations thereof. It will be understood that removal of reactants from the reaction space can be a relative action and can be understood as movement of excess reactants in relation to the vicinity of the substrate; for example, in space-divided ALD moving the substrate from the zone effectively moves the reaction space associated with the substrate, leaving the reactants of the prior phase behind in a different reaction zone. In the next block 30, the substrate is contacted with excited species, which react with the adsorbed species on the substrate. The phase of plasma ALD in which excited species are supplied can be referred to as a “plasma phase,” although plasma discharge is not always employed to create the excited species, and even when an actual plasma discharge is created, it may be remote from the substrate and plasma products are supplied to a downstream substrate. For simplicity, the term “excited species” used herein can be understood to encompass electrons, ions, radicals, atoms or other excited species that can, for example, be generated by a plasma. Typically the excited species are formed in a plasma discharge and depending on how they are supplied to the reaction space where substrate is loaded the excited species may comprise electrons, ions, radicals and/or atoms, for example oxygen, hydrogen or nitrogen plasma, ions, radicals, atomic oxygen/hydrogen/nitrogen, or other excited species that can, for example, be generated by a plasma. Thus some excited species such as O, H and N can be electrically neutral. In some embodiments the excited species does not comprise hydrogen. In some embodiments the excited species comprise only nitrogen. In some embodiments the excited species comprise only oxygen. Skilled artisan will understand that, for example, during plasma discharge additional gases may be present in addition to the excited species, such as rare gases like He, Ne, Ar to help in plasma ignition or otherwise make the process better like more stable and repeatable, but these species are considered not to be significant contributors to the film growth.
Excited species may be generated in situ in the reaction chamber, or may be supplied from a remote plasma unit (RPU) or the like. In various embodiments excited species may be generated by coupling power, such as by RF alternated electrical fields, microwave standing waves, ultraviolet light, or other forms of energy, to a flowing vapor phase reactant. The excited species reaction with the adsorbed species may strip ligands from adsorbed species to prepare the surface for subsequent reactants, and may additionally contribute elements to the film. In block 40, excess excited species are removed from the reaction space. Such removal can be accomplished, e.g., by turning off the power that generates the excited species, and by physical removal as in block 20, e.g., by purging, pump down, moving the substrate away from a zone in which the excited species is supplied, or combinations thereof. In some embodiments, the excited species is formed from gases that are inert under the deposition conditions in the absence of excitement, such as N2 or O2, depending upon the reactivity of the adsorbed species. Limiting residence time as disclosed below aids in more quickly eliminating active species in block 40 after the plasma power is removed.
The blocks 10-40 together define a cycle 50, which can be repeated until a film of the desired thickness is left on the substrate. As noted above, the cycle 50 can include additional reactant supply blocks (not shown), and need not be identically performed in each repetition. For example, other reactant(s) can be introduced in separate phase(s) in each cycle; other reactant(s) can be introduced in separate phase(s) every few cycles to incorporate a controlled amount of another element; other reactant(s) can be introduced in separate phase(s) in each cycle or every few cycles for gettering; separate reactants can be provided for stripping ligands from the adsorbed species and for contributing additional elements; etc.
The techniques taught herein can be applied to plasma enhanced or assisted ALD in a wide variety of reactor configurations.
In general plasma ALD reactors can be configured for single substrates or for multiple substrates. In some arrangements, multiple substrates are stacked vertically; however, in order to maximize effectiveness of the excited species, multiple substrate reactors preferably array the substrates adjacent to one another, similar to the enlarged platform arrangement of
As noted above, the skilled artisan may expect an ALD process to be optimized by altering conditions to more efficiently achieve saturation of surface reactions. For example, if an unacceptably low growth rate per cycle or high impurity level is found, more efficient reactions may be expected from, e.g., prolonging a reactant exposure step or increasing substrate temperatures, as long as temperature remain in suitable regime (e.g., below the thermal decomposition temperature of reactants). Thus, conventional parameters modulated include temperature, pressure, reactant supply rates and reactant exposure durations. In plasma processing, plasma power may also be modulated.
It has been found that, for plasma phases of plasma ALD processes, modulation of reactant residence time in the process chamber can have a significant impact on film quality for plasma ALD. Without being limited by theory, it is possible that the more reactive species derived from plasma or otherwise excited can cause interactions within the reaction space that lead to redeposited species. For example, it is possible that ligands removed from the adsorbed species of a prior phase can interact with the energetic species still in the reaction space, can form new species, which can then interact with the substrate surface again and occupy reaction sites that would otherwise be available for the next ALD phase. Such redeposition can cause the process to take longer to remove ligands and byproduct from the substrate surface. Modulation of residence time, particularly reducing residence time by increasing the speed of the plasma products' movement through the reaction space, and limit the potential for redeposition and obtain more complete surface reactions, leaving fewer undesired impurities from unremoved or redeposited ligands and/or more dense films.
The residence time τ is defined as
where V is the volume of the reaction space and S is the effective volumetric pumping speed for the vacuum pump exhausting the reaction space. The residence time τ is an indication of how long the relevant species spend inside the reactor before being removed to the exhaust. It represents the 1/e time, or average time for reduction of the relevant species in the reaction space by 63.2%, rather than an absolute limit for every molecule of the relevant species.
The residence time can be varied by varying the effective pumping speed, where the volume of the reactor can be considered fixed. The effective pumping speed can be varied by changing the pump or its operating conditions. For example, the rotation speed of pumps can be varied, such as rotation speed of turbo pumps. The effective pumping speed also depends on the conductance of the pump line so that is also a hardware adjustment that can be used to change the effective pumping speed. Residence time can also be modulated by controlling valves between the reactor and pump, e.g. by partly closing an exhaust valve partly or by using a butterfly valve, and can be adjusted through the operating software of the reactor. The effective pumping speed can also depend upon the pressure inside the reactor so by changing the pressure, for example by changing the overall gas inlet flows, the effective pumping speed can also be varied. Moreover, different gases in the gas mixture can exhibit different effective pumping speeds where all other parameters are kept constant. The skilled artisan can determine how changing such additional variables can affect the effective pumping speed S for calculation of the residence time.
In some embodiments, residence time for the excited species in the plasma phase of the plasma ALD process can be optimized to minimize impurities in the deposited film, or to maximize film density. In some embodiments, impurity levels are kept below about 5 atomic %, preferably below about 2 atomic %, and more preferably below about 1%. In some examples, optimization can be performed using the principles taught herein to achieve impurity levels below about 0.5 atomic %. “Impurities” refer to elements present in the ALD reactants (both plasma and non-plasma reactants) that are not desired in the film, and the percentages provided above represent total impurity percentages in the deposited film, and therefore can also represent maximum impurity levels for each contaminant present in the precursors. For all materials hydrogen can be excluded from the definition of impurities as it is somewhat difficult to analyze accurately for very thin films. For example, for silicon oxide or metal oxides, impurities to be minimized include halides, carbon and nitrogen (to the extent these elements are present in the reactants). For silicon nitride or metal nitrides, impurities to be minimized include halides, carbon and oxygen (to the extent these elements are present in the reactants).\
In other arrangements, residence time for the excited species in the plasma phase of the plasma ALD process can be optimized to maximize an indicator of film density. The nitrogen plasma residence time for silicon nitride plasma ALD recipes in the examples below, for example, can be optimized to produce films with index of refractions greater than about 1.9, and preferably greater than about 1.95. Similarly, the nitrogen plasma residence time for silicon nitride plasma ALD can be optimized to produce films with low wet etch rates, for example, wet etch rates in a buffered, 7:1 dilute HF solution can be less than about 1.5 nm/min, preferably less than about 1.0 nm/min and more preferably less than about 0.7 nm/min.
At the same, in keeping with general advantages for ALD, plasma ALD processes with minimized residence time, as taught herein affords highly conformal layers over topography, relative to non-ALD deposition techniques. Conformality is typically measured in terms of step coverage over features on the substrate, and can either be measured as a ratio of deposited thickness on sidewalls to deposited thickness on top surfaces (S/T), or as a ratio of deposited thickness on bottom surfaces to deposited thickness on top surfaces (B/T). Under either measure, the processes taught herein can afford step coverage of more than about 75%, preferably more than about 90%, more preferably more than about 95% and in some cases more than about 99%. These ratios can hold true over substrates with features having height-to-width aspect ratios (AR) of about 2:1 or greater, preferably about 5:1 or greater, and even about 8:1 and greater.
In some embodiments, residence time for the excited species in the reaction space is less than about 1.0 s. Preferably the residence time is less than 0.5 s, more preferably less than about 0.2 s. In some embodiments, residence time may be below about 0.05 s and if carefully optimized residence times below about 0.01 s can be achieved. Depending on the reaction space volume, the effective pumping speed to accomplish such residence times can vary. For most single substrate reactors, or multi-substrate reactors with zones sizes for individual substrates (similar to
While the residence time for the excited species is kept relatively low, representing a relative rapid rate of flow through the reaction space, the duration of the plasma phase is desirably kept long enough to ensure saturative reaction of the excited species with the substrate surface. The plasma phase duration is the time during which the excited species is supplied to the substrate while plasma or other exciting power is coupled to the gas from which the excited species is generated. In some embodiments, the plasma phase can have a duration greater than about 0.05 s. Preferably the plasma phase has a duration greater than about 0.1 s, more preferably greater than about 0.2 s or 0.5 s. While lengthening the cycle duration may not be economical in terms of throughput, higher quality films can be more important in some situations, particularly where very thin, conformal layers are desired. However, most reactors will have practical limits on the duration of the plasma phase, such as the need to avoid overheating the substrates and/or equipment. Typically single substrate plasma ALD reactors employ plasma phase durations of less than about 10 s.
The teachings herein with respect to residence time can be applied to a number of different plasma ALD recipes, including recipes in which excited nitrogen, hydrogen or oxygen species are provided in the plasma phase(s) of the plasma ALD process. Specific examples are provided below for silicon nitride (SiN). Examples of insulating films include SiN, silicon oxide (SiO), mixtures of SiN and SiO (SiON), aluminum nitride (AlN), etc., where the above abbreviations encompass a wide variety of atomic ratios and do not necessarily represent stoichiometric materials. Other examples of insulating films include high-k films such as ZrO2, HfO2, Al2O3, Ta2O5, etc., as well as mixtures and non-stoichiometric forms of the above. The principles taught herein can also be applied to conductive films, such as transition metal nitrides, carbides, carbonitrides, borides and mixtures thereof, where plasma phases can supply excited nitrogen, hydrogen, carbon and/or boron species. Furthermore, excited oxygen species are also useful for conductive oxides such as RuO2, IrO2, SnO2, etc.
In the experiments, silicon nitride was deposited by a first phase including exposing the substrate to an organic silicon precursor that adsorbs on the substrate surface; followed by stopping provision of the silicon precursor to the substrate; followed by a second phase including exposing the substrate to excited nitrogen species that reacted with the adsorbed silicon species from the first phase; followed by stopping provision of the silicon precursor. It will be understood that, because the plasma ALD process is cyclical, the “first” phase need not be the first step in the process. In the experiments, stopping the provision of a reactant included both stopping the flow of the reactant to the reaction space and removal of excess reactant from the substrate surface by provision of inert purge gas through the reaction space. In the case of the plasma phase, the inert purge gas can be a continuation of N2 gas after plasma power is removed from the flow, and purge gas can additionally be supplied through the inlet for the silicon precursor. In space-divided ALD embodiments, stopping the provision of a reactant can involve moving the substrate out of the silicon precursor zone, and moving the substrate through a flowing inert gas (e.g., a purge gas curtain or another zone supplied with purge gas) can additionally remove excess excited species from the substrate.
The excited nitrogen species can be provided by coupling power to a nitrogen source gas alone (especially N2), a nitrogen source and hydrogen (e.g., N2+H2), or a nitrogen source and noble gas for supporting plasma generation (e.g., NH3+Ar, He or Ne). Preferably nitrogen plasma includes supply of N2 without noble gases.
Preferably, the silicon precursor is an aminosilane or an aminesilane. In some embodiments the silicon precursor comprises a silicon amine, where silicon is bonded to two nitrogen atoms and two hydrogen atoms. For example, the silicon precursor may comprise bis(dialkylamine)silane, (R2N)2Si—H2. In some embodiments the silicon precursor comprises BDEAS (=bis(diethylamino)silane). In some embodiments the silicon precursor comprises a silicon amine, where silicon is bonded to three nitrogen atoms and one hydrogen atom. For example, the silicon precursor may comprise tris(dialkylamine)silane, (R2N)3Si—H1. In some embodiments, the silicon precursor comprises a silicon amine, where silicon is bonded to four nitrogen atoms. For example, the silicon precursor may comprise tetrakis(dialkylamine)silane, (R2N)4Si. In some embodiments, the silicon precursor comprises aminosilane, where the silicon is bonded to one nitrogen atom and three hydrogen atoms. For example, the silicon precursor may comprise dialkylaminesilane, (R2N)Si—H3.
Organic compounds having a Si—Si bond and an NHx group either attached directly to silicon (to one or more silicon atoms) or to a carbon chain attached to silicon are used in some embodiments. In some embodiments, the silicon precursor may comprise an aminodisilane, such as hexakis(ethylamino)disilane. In some embodiments the silicon compound may have the formula:
RIII3-x(RIIRIN)xSi—Si(N—RIRII)yRIII3-y
wherein:
In some embodiments the silicon compound is hexakis(monoalkylamino)disilane:
(RII—NH)3Si—Si(NH—RII)3
In other embodiments the silicon compound is (CH3—O)3Si—Si(O—CH3)3
In still other embodiments, the silicon precursor is a halide, such as a silicon chloride. Examples include but are not limited to octachlorotrisilane (Si3Cl8, OCTS); hexachlorodisilane (Si2Cl6, HCDS); and dichlorosilane (SiH2Cl2, DCS).
In the experiments, a silicon amine, and particularly SiH2(NHtBu)2, also referred to as BTBAS, was employed in alternation with products of a nitrogen-containing plasma, particularly a plasma generated from N2 gas. A variety of plasma ALD conditions were applied, including substrate temperatures from about 100° C. to about 500° C., chamber pressures from about 10 mTorr to about 100 mTorr, and plasma exposure times from about 2 seconds to about 20 seconds.
However, the shorter residence time for the gases during the plasma phase in the process used for
Although certain embodiments and examples have been discussed, it will be understood by those skilled in the art that the scope of the claims extend beyond the specifically disclosed embodiments to other alternative embodiments and/or uses and obvious modifications and equivalents thereof.
The present application is a continuation of U.S. application Ser. No. 15/499,188, filed Apr. 27, 2017, which is a continuation of U.S. application Ser. No. 14/231,317 filed Mar. 31, 2014, now U.S. Pat. No. 9,637,823, which are hereby incorporated by reference in their entirety.
| Number | Name | Date | Kind |
|---|---|---|---|
| 9637823 | Knoops | May 2017 | B2 |
| 10072337 | Knoops | Sep 2018 | B2 |
| 20050009325 | Chung et al. | Jan 2005 | A1 |
| 20050042865 | Cabral et al. | Feb 2005 | A1 |
| 20090155606 | Yoon et al. | Jun 2009 | A1 |
| 20120045589 | Ivanov et al. | Feb 2012 | A1 |
| 20150004805 | Omstead et al. | Jan 2015 | A1 |
| 20150017812 | Chandrasekharan et al. | Jan 2015 | A1 |
| 20150021599 | Ridgeway et al. | Jan 2015 | A1 |
| 20150031218 | Karakawa | Jan 2015 | A1 |
| Entry |
|---|
| Knoops, et al. “Reaction Mechanisms of Atomic Layer Deposition of TaNx from Ta(NMe2)5 Precursor and H2-based Plasmas,” J. Vac. Sci. Technol. A, vol. 30, No. 1, 01A101-1-01A101-10, 2012. |
| Knoops, et al. “Plasma-assisted ALD of Silicon Nitride from BTBAS,” 13th International Conference on Atomic Layer Deposition, Jul. 28-31, 2013, San Diego, California, U.S.A., 21 pages. |
| Number | Date | Country | |
|---|---|---|---|
| 20180363143 A1 | Dec 2018 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 15499188 | Apr 2017 | US |
| Child | 16116321 | US | |
| Parent | 14231317 | Mar 2014 | US |