The present application claims priority from Japanese Patent Application No. 2017-154942 filed on Aug. 10, 2017, the content of which is hereby incorporated by reference into this application.
The present invention relates to an atomic layer deposition apparatus, a film-forming method using an atomic layer deposition apparatus, and a cleaning method of an atomic layer deposition apparatus.
Japanese Patent Application Laid-Open Publication No. 2002-280376 (Patent Document 1) describes a cleaning method of a CVD (Chemical Vapor Deposition) apparatus having a shower head.
Japanese Patent Application Laid-Open Publication No. 2014-210946 (Patent Document 2) describes a technique relating to an atomic layer deposition apparatus.
The atomic layer deposition method is a film-forming method in which a film is formed in a unit of atomic layer over a substrate by alternately supplying source gas and reaction gas onto the substrate. Since the atomic layer deposition method forms a film in a unit of atomic layer, it has an advantage of excellent step coverage and film thickness controllability. On the other hand, in an atomic layer deposition apparatus that embodies the atomic layer deposition method, a film is likely to be formed at a place where the film is difficult to remove as a flip side of the advantage of excellent step coverage. For this reason, in the atomic layer deposition apparatus, there is concern that generation of a foreign matter caused by peeling of the film formed at the place where the film is difficult to remove may deteriorate the quality of the film formed over the substrate.
Other problems and novel features of the present invention will be apparent from the description of the present specification and the accompanying drawings.
An atomic layer deposition apparatus according to an embodiment includes: a cleaning gas supply port provided on a first side wall of a film-forming container; and a cleaning gas exhaust port provided on a second side wall opposed to the first side wall of the film-forming container.
According to an embodiment, it is possible to suppress the deterioration of quality of the film formed over the substrate.
The same components are denoted by the same reference characters throughout the drawings for describing the embodiments in principle, and the repetitive description thereof will be omitted. Also, hatching is sometimes used even in a plan view so as to make the drawing easy to see.
<Unique Circumstances to Atomic Layer Deposition Apparatus>
For example, in a plasma CVD apparatus, a plasma discharge is generated between a lower electrode which holds a substrate and an upper electrode opposed to the lower electrode while supplying a plurality of source gases between the lower electrode and the upper electrode. In this manner, in the plasma CVD apparatus, a film is formed over the substrate by the chemical reaction caused by active species (radicals) generated by the plasma discharge. At this time, in the plasma CVD apparatus, the film is mainly formed in a region (discharge space) in which the plasma discharge is generated. This is because source gas having a property of being difficult to diffuse is used as the source gas used in the plasma CVD apparatus in order to localize the gas in the discharge space and a film material is formed only after active species (radicals) are generated by the plasma discharge from a plurality of source gases. Therefore, in the plasma CVD apparatus, a film is less likely to be formed at a place away from the discharge space (place where no plasma discharge is generated).
On the other hand, in the plasma atomic layer deposition apparatus, a film is formed in a unit of atomic layer over a substrate by alternately supplying source gas and reaction gas between a lower electrode which holds the substrate and an upper electrode opposed to the lower electrode and performing plasma discharge when supplying the reaction gas. At this time, in the plasma atomic layer deposition apparatus, the film with excellent step coverage can be formed by forming the film in a unit of atomic layer. Particularly, in the plasma atomic layer deposition apparatus, in order to improve the step coverage, a material which easily diffuses is used as source gas, and each of the gases (source gas, purge gas, and reaction gas) is alternately supplied while securing the time enough for each gas to diffuse sufficiently in a film-forming container. Therefore, the source gas and the reaction gas are distributed not only over the substrate but also to every corner of the film-forming container. Further, in the plasma atomic layer deposition apparatus, active species (radicals) are generated by the plasma discharge of the reaction gas and a film is formed by the reaction between the active species and the source gas adsorbed over the substrate, whereas the source gas and the reaction gas are likely to react with each other even in a state where the active species (radicals) are not generated by the plasma discharge. Therefore, in the plasma atomic layer deposition apparatus, the source gas and the reaction gas react with each other to form a film also in a small gap of the film-forming container where no plasma discharge is generated. In other words, since the atomic layer deposition apparatus has the features of: (1) a film is formed in a unit of atomic layer; (2) the source gas and the reaction gas are distributed to every corner of the film-forming container; and (3) the source gas and the reaction gas are likely to react with each other even in a place where no plasma discharge is generated, the film is formed also in a small gap.
As described above, the plasma atomic layer deposition apparatus has a characteristic that the film is formed not only over the substrate but also at every corner in the film-forming container including a small gap. Thus, in the following, a related art of the plasma atomic layer deposition apparatus will be first described. Thereafter, the room for improvement present in the related art will be described, and then, a plasma atomic layer deposition apparatus according to the first embodiment will be described.
<Description of Related Art>
Next, as shown in
In the plasma atomic layer deposition apparatus 100 according to a related art configured as described above, a film is formed over the substrate 10 by performing the operations shown below. First, source gas is supplied from the source gas supply unit (not shown) through the source gas supply path 106A, the injector 106, and the source gas supply port 104 to the film-forming space 103 of the film-forming container 100A. Then, the source gas supplied to the film-forming space 103 is exhausted from the exhaust unit 108 through the gas exhaust port 105 and the gas exhaust path 107. Subsequently, purge gas is supplied from the purge gas supply unit (not shown) through the purge gas supply path 106B, the injector 106, and the source gas supply port 104 to the film-forming space 103 of the film-forming container 100A. Then, the purge gas supplied to the film-forming space 103 is exhausted from the exhaust unit 108 through the gas exhaust port 105 and the gas exhaust path 107. In this manner, the remaining source gas can be removed by the purge gas. Subsequently, reaction gas is supplied from the reaction gas supply unit (not shown) through the reaction gas supply path 106C, the injector 106, and the source gas supply port 104 to the film-forming space 103 of the film-forming container 100A. At this time, a high frequency voltage is applied between the lower electrode 101 and the upper electrode 102. As a result, the reaction gas supplied to the film-forming space 103 sandwiched between the lower electrode 101 and the upper electrode 102 is turned into plasma. In this manner, a film is formed over the substrate 10. Thereafter, purge gas is supplied from the purge gas supply unit (not shown) through the purge gas supply path 106D, the injector 106, and the source gas supply port 104 to the film-forming space 103 of the film-forming container 100A. Then, the purge gas supplied to the film-forming space 103 is exhausted from the exhaust unit 108 through the gas exhaust port 105 and the gas exhaust path 107. In this manner, the remaining reaction gas can be removed by the purge gas. The film can be formed over the substrate 10 by operating the plasma atomic layer deposition apparatus 100 according to the related art in the manner described above.
<Consideration for Improvement>
Here, as described in the part of <Unique Circumstances to Atomic Layer Deposition Apparatus>, the plasma atomic layer deposition apparatus has a characteristic that the film is formed not only over the substrate but also at every corner in the film-forming container including a small gap.
Particularly, as shown in
<Configuration of Plasma Atomic Layer Deposition Apparatus>
Further, as shown in
As described above, the plasma atomic layer deposition apparatus 1 according to the first embodiment includes the film-forming container 1A, the lower electrode 11 arranged on a lower surface of the film-forming container 1A, and the upper electrode 12 arranged on an upper surface of the film-forming container 1A for generating plasma discharge with the lower electrode 11. Also, the plasma atomic layer deposition apparatus 1 according to the first embodiment includes a source gas supply port 14 provided on a side surface 200A (side wall on the left side of
Next, as shown in
<Atomic Layer Deposition Method>
The plasma atomic layer deposition apparatus 1 according to the first embodiment is configured as described above, and an atomic layer deposition method using the plasma atomic layer deposition apparatus 1 according to the first embodiment will be described below.
First, after preparing the substrate 10 shown in
Subsequently, after the supply of the source gas stops, purge gas is supplied from the purge gas supply unit into the film-forming container 1A through the purge gas supply path 16B, the injector 16, and the source gas supply port 14 (S103 in
Next, reaction gas is supplied from the reaction gas supply unit into the film-forming container 1A through the reaction gas supply path 16C, the injector 16, and the source gas supply port 14 (S104 in
Subsequently, after the supply of the reaction gas stops, purge gas is supplied from the purge gas supply unit through the purge gas supply path 16D, the injector 16, and the source gas supply port 14 into the film-forming container 1A (S106 in
In the above-described manner, a thin layer made of a single atomic layer ATL is formed over the substrate 10. Then, by repeating the above-described steps (S102 to S105 in
Next, features in the first embodiment will be described. The first feature in the first embodiment is that the lower adhesion preventing member 19A is provided between the lower space 110 located below the lower electrode 11 and the film-forming space 13 located above the lower electrode 11 as shown in, for example,
For example, as described in the part of <Unique Circumstances to Atomic Layer Deposition Apparatus>, the plasma atomic layer deposition apparatus has a characteristic that the film is formed not only over the substrate but also at every corner in the film-forming container including a small gap. Therefore, when the lower space 110 of the lower electrode (stage) 101 communicates with the film-forming space 103 like in the plasma atomic layer deposition apparatus 100 according to the related art shown in
In this regard, in the plasma atomic layer deposition apparatus 1 according to the first embodiment shown in
However, even when the lower space 110 located below the lower electrode 11 is separated from the film-forming space 13 by the lower adhesion preventing member 19A, since the plasma atomic layer deposition method has a characteristic that the film is likely to be formed also in a small gap, if a minute gap is present between the lower adhesion preventing member 19A and the lower electrode 11, the source gas and the reaction gas may enter the lower space 110 through the minute gap. At this time, even when the lower space 110 located below the lower electrode 11 is separated from the film-forming space 13 by the lower adhesion preventing member 19A, if the pressure in the lower space 110 is lower than the pressure in the film-forming space 13, the potential that the source gas and the reaction gas flow into the lower space with lower pressure from the film-forming space 13 with higher pressure through the minute gap present between the lower adhesion preventing member 19A and the stage (lower electrode 11) is increased.
For example, the source gas, the reaction gas, and the purge gas are supplied to the film-forming space 13, while the source gas, the reaction gas, and the purge gas are not supplied to the lower space 110 separated from the film-forming space 13 by the lower adhesion preventing member 19A. Therefore, if no measures are taken, it is inevitable that the pressure in the lower space 110 will be lower than the pressure in the film-forming space 13. Accordingly, in the case where the pressure in the lower space 110 is lower than the pressure in the film-forming space 13, even if the first feature in the first embodiment described above is adopted, there is probability that the unnecessary film is formed on the member in contact with the lower space 110. Thus, on the premise that the first feature of separating the lower space 110 from the film-forming space 13 by the lower adhesion preventing member 19A is adopted, making the pressure in the lower space 110 higher than the pressure in the film-forming space 13 may be conceivable. However, when the pressure in the lower space 110 is made higher than the pressure in the film-forming space 13, the potential that the foreign matter which is present in the lower space 110 enters the film-forming space 13 for some reasons is increased. Thus, in the plasma atomic layer deposition apparatus 1 according to the first embodiment, on the premise that the first feature of separating the lower space 110 from the film-forming space 13 by the lower adhesion preventing member 19A is adopted, the pressure in the lower space 110 is made equal to the pressure in the film-forming space 13. Namely, the second feature in the first embodiment is that the pressure in the lower space 110 is made equal to the pressure in the film-forming space 13 on the premise of the above-described first feature. Thus, according to the second feature in the first embodiment, it is possible to further lower the potential that the source gas and the reaction gas flow into the lower space 110 while keeping the advantages of the first feature described above, and also possible to reduce the potential that the foreign matter flows from the lower space 110 into the film-forming space 13.
From the above, in the case of adopting the first feature and the second feature in the first embodiment, it is possible to effectively improve the quality of the film to be formed over the substrate 10 by the synergistic effect brought by the first feature and the second feature.
Subsequently, the third feature in the first embodiment is that the upper adhesion preventing member 19B is attached to the opposing surface (lower surface) of the upper electrode 12 opposed to the lower electrode 11 as shown in
For example, when the upper adhesion preventing member 19B is not attached to the upper electrode 12 itself, an unnecessary film is formed over the upper electrode 12 itself. In this case, the film is peeled off from the upper electrode 12 itself to generate a foreign matter, and this foreign matter is deposited onto the substrate 10 mounted on the lower electrode 11 positioned below the upper electrode 12. As a result, the foreign matter adheres to the substrate 10, so that the quality of the film formed over the substrate 10 is deteriorated. For this reason, it is necessary to remove the unnecessary film formed on the upper electrode 12 itself in order to suppress the deterioration of quality of the film formed over the substrate 10.
Here, for example, it is conceivable to detach the upper electrode 12 itself from the plasma atomic layer deposition apparatus 1 and then remove the unnecessary film adhered to the upper electrode 12 by wet etching. However, when the upper electrode 12 detached from the plasma atomic layer deposition apparatus 1 is subjected to wet etching and the upper electrode 12 is attached to the plasma atomic layer deposition apparatus 1 again, the attachment position of the upper electrode 12 becomes different from the previous attachment position. In this case, the state of the plasma discharge between the upper electrode 12 and the lower electrode 11 changes. In other words, in the method of detaching the upper electrode 12 and removing the unnecessary film formed on the upper electrode 12 by wet etching, the attachment position of the upper electrode 12 itself cannot be reproduced, so that the attachment position of the upper electrode 12 changes, resulting in that the film forming conditions represented by the state of plasma discharge may change. In this case, there is the possibility that the quality of the film formed over the substrate 10 may be fluctuated. Further, in the method of removing the unnecessary film adhered to the upper electrode 12 itself by wet etching, it is necessary to detach the upper electrode 12 from the film-forming container 1A of the plasma atomic layer deposition apparatus 1 after the interior of the film-forming container 1A is released to the atmospheric pressure, which leads to decrease in maintenance workability.
Accordingly, in the first embodiment, the upper adhesion preventing member 19B is attached to the opposing surface (lower surface) of the upper electrode 12 opposed to the lower electrode 11. Thus, according to the first embodiment, it is possible to suppress the unnecessary film from being formed on the upper electrode 12 itself. Namely, when the third feature in the first embodiment is adopted, the unnecessary film is not formed on the upper electrode 12 itself but is formed on the upper adhesion preventing member 19B attached to the upper electrode 12. In this case, the upper adhesion preventing member 19B having the unnecessary film formed thereon is detached from the upper electrode 12, and the unnecessary film formed on the upper adhesion preventing member 19B is removed. In other words, according to the third feature in the first embodiment, since it is not necessary to detach the upper electrode 12 itself from the plasma atomic layer deposition apparatus 1, it is possible to reduce the occurrence potential of the foreign matter without causing the change in the film forming conditions represented by the plasma discharge condition. Namely, according to the third feature in the first embodiment, it is possible to reduce the occurrence potential of the foreign matter while suppressing the fluctuation in the quality of the film formed over the substrate 10 due to the change in the film forming conditions. Furthermore, according to the third feature in the first embodiment, since it is only necessary to detach the upper adhesion preventing member 19B from the upper electrode 12 and it is not necessary to detach the upper electrode 12 itself from the plasma atomic layer deposition apparatus 1, it is possible to achieve the remarkable effect that the maintenance workability can be improved.
Next, the fourth feature in the first embodiment is that the lower adhesion preventing member 19A and the upper adhesion preventing member 19B are arranged in parallel to each other such that the gas flow in the film-forming space 13 is smoothed. Particularly, in the atomic layer deposition method, it is important to smoothly supply the gases (source gas, purge gas, reaction gas) to the film-forming space 13 and exhaust the gases (source gas, purge gas, reaction gas) from the film-forming space 13 in order to improve the film thickness uniformity of the film formed over the substrate 10. Furthermore, it is important to increase the conductance indicating the gas flowability in order to achieve satisfactory film formation in a unit of atomic layer by the atomic layer deposition method.
In this regard, for example, in the plasma atomic layer deposition apparatus 100 according to the related art shown in
On the other hand, in the plasma atomic layer deposition apparatus 1 according to the first embodiment, for example, the lower adhesion preventing member 19A that closes the lower space 110 and the upper adhesion preventing member 19B that is attached to the opposing surface (lower surface) of the upper electrode 12 are arranged in parallel to each other as shown in
In the first embodiment, the technical idea in which the occurrence potential of the foreign matter in the film-forming container is reduced by suppressing the formation of the unnecessary film on the member in contact with the lower space, thereby improving the quality of the film formed over the substrate has been described. In the second embodiment, the technical idea in which the occurrence potential of the foreign matter in the film-forming container is reduced by further removing the unnecessary film formed in the film-forming container, thereby improving the quality of the film formed over the substrate, while adopting the configuration of the plasma atomic layer deposition apparatus 1 according to the first embodiment, will be described. Specifically, in the second embodiment, an example in which a cleaning mechanism is provided in the plasma atomic layer deposition apparatus according to the first embodiment will be described.
In
In the plasma atomic layer deposition apparatus 1 according to the second embodiment, the unnecessary film formed on the member in contact with the film-forming space 13 chemically reacts with the fluorine radicals contained in the cleaning gas to be gasified, and the gasified product is exhausted from the film-forming space 13 to the outside of the film-forming container 1A through the exhaust unit 18. As a result, in the plasma atomic layer deposition apparatus 1 according to the second embodiment, the unnecessary film formed in the film-forming container 1A can be removed. Therefore, in the plasma atomic layer deposition apparatus 1 according to the second embodiment, the unnecessary film formed in the film-forming container 1A can be removed by the cleaning gas containing fluorine radicals, so that the occurrence potential of the foreign matter in the film-forming container 1A can be reduced. Thus, in the plasma atomic layer deposition apparatus 1 according to the second embodiment, it is possible to improve the quality of the film formed over the substrate 10. In other words, in the plasma atomic layer deposition apparatus 1 according to the second embodiment, the occurrence potential of the foreign matter in the film-forming container 1A can be reduced by the synergistic effect of the approach in the first embodiment in which the formation of the unnecessary film on the member in contact with the lower space is suppressed and the approach in which the unnecessary film formed in the film-forming container 1A is removed by the cleaning gas containing fluorine radicals. Therefore, according to the second embodiment, the quality of the film formed over the substrate 10 can be improved.
Next, features in the second embodiment will be described. The fifth feature in the second embodiment is that cleaning gas containing fluorine radicals is generated by turning cleaning gas into plasma in the cleaning gas supply unit 30 provided outside the film-forming container 1A and then the cleaning gas containing fluorine radicals is introduced into the film-forming space 13 in the film-forming container 1A as shown in
Thus, according to the second embodiment, it is possible to effectively remove the unnecessary film formed at every corner of the film-forming container 1A.
Note that the term “remote plasma” used in the present specification means the configuration mode in which plasma is not generated inside the film-forming container 1A but is generated in the plasma supply unit provided outside the film-forming container 1A and the plasma generated in the plasma supply unit is supplied into the film-forming container 1A.
Here, for example, it is conceivable that the cleaning gas is turned into plasma by applying a high frequency voltage between the lower electrode 11 and the upper electrode 12 arranged in the film-forming container 1A after introducing the cleaning gas into the film-forming container 1A, thereby performing the cleaning in the film-forming container 1A. In this case, however, the cleaning gas turned into plasma is locally present only in the film-forming space 13 sandwiched between the lower electrode 11 and the upper electrode 12 in the film-forming container 1A. Therefore, in this cleaning method, the unnecessary film adhered to the member present in the vicinity of the film-forming space 13 sandwiched between the lower electrode 11 and the upper electrode 12 can be removed, but it is difficult to sufficiently remove the unnecessary film formed at every corner of the film-forming container 1A away from the film-forming space 13. This is because the cleaning gas turned into plasma is locally present in the vicinity of the film-forming space 13 sandwiched between the lower electrode 11 and the upper electrode 12 and thus the cleaning gas turned into plasma does not reach the corner portions of the film-forming container 1A. In particular, as described in the part of <Unique Circumstances to Atomic Layer Deposition Apparatus>, the plasma atomic layer deposition apparatus 1 has a characteristic that the film is formed not only over the substrate 10 but also at every corner in the film-forming container 1A including a small gap. Therefore, it is important to perform the cleaning up to every corner portion in the film-forming container 1A in the plasma atomic layer deposition apparatus 1. In this regard, it is difficult to perform the cleaning up to every corner portion in the film-forming container 1A in the cleaning method in which cleaning gas is turned into plasma by applying a high frequency voltage between the lower electrode 11 and the upper electrode 12 arranged in the film-forming container 1A, thereby performing the cleaning inside the film-forming container 1A. Namely, it cannot be said that this cleaning method is sufficient for realizing the technical idea in which the occurrence potential of the foreign matter in the film-forming container 1A is reduced by removing the unnecessary film formed in the film-forming container 1A, thereby improving the quality of the film formed over the substrate 10.
On the other hand, according to the fifth feature in the second embodiment in which the cleaning in the film-forming container 1A is performed by using the so-called remote plasma, it is possible to sufficiently remove the unnecessary film formed at every corner of the film-forming container 1A away from the film-forming space 13. This is because since the cleaning gas in which the fluorine radicals have been generated in advance is introduced into the film-forming container 1A in the cleaning method using the remote plasma, the cleaning gas containing fluorine radicals can be distributed to every corner of the film-forming container 1A, as compared with the cleaning method in which the cleaning gas is turned into plasma in the film-forming container 1A. Thus, in the cleaning method according the second embodiment, the unnecessary film formed at the corner portions of the film-forming container 1A can be sufficiently removed. From the above, it can be said that the cleaning method according to the second embodiment using the remote plasma is sufficient for realizing the technical idea in which the occurrence potential of the foreign matter in the film-forming container 1A is reduced by removing the unnecessary film formed in the film-forming container 1A, thereby improving the quality of the film formed over the substrate 10.
Subsequently, the sixth feature according to the second embodiment is that the cleaning gas containing fluorine radicals is introduced into the film-forming container 1A in a lateral direction and the cleaning gas containing fluorine radicals is exhausted to the outside of the film-forming container 1A in the lateral direction as shown in
For example, assuming that the cleaning method using the remote plasma is adopted, the configuration in which the cleaning gas containing fluorine radicals is introduced into the film-forming container 1A from an upper part of the film-forming container 1A is conceivable. However, when the cleaning gas containing fluorine radicals is introduced into the film-forming container 1A from an upper part of the film-forming container 1A, it is inevitable that the cleaning gas containing fluorine radicals is diffused in the lateral direction of the film-forming container 1A after being blown onto the stage including the lower electrode 11. At this time, the fluorine radicals have the property of being deactivated when they hit an obstacle such as the stage. For example, when the fluorine radicals in an active state are distributed to every corner portion of the film-forming container 1A, the reaction between the fluorine radicals in an active state and the unnecessary film formed at the corner portions of the film-forming container 1A is promoted, and it is thus possible to sufficiently remove the unnecessary film formed at the corner portions of the film-forming container 1A. On the other hand, when the fluorine radicals are deactivated, even if the fluorine radicals are distributed to every corner portion of the film-forming container 1A, the reaction between the fluorine radicals in a deactivated state and the unnecessary film formed at the corner portions of the film-forming container 1A is less likely to be promoted, and it is thus not possible to sufficiently remove the unnecessary film formed at the corner portions of the film-forming container 1A. Accordingly, in the cleaning method in which the cleaning gas containing fluorine radicals is introduced into the film-forming container 1A from an upper part of the film-forming container 1A, it is not possible to sufficiently remove the unnecessary film formed at the corner portions of the film-forming container 1A.
On the other hand, in the cleaning method according to the second embodiment in which the cleaning gas containing fluorine radicals is introduced into the film-forming container 1A in a lateral direction and the cleaning gas containing fluorine radicals is exhausted to the outside of the film-forming container 1A in the lateral direction, the cleaning gas containing fluorine radials does not hit an obstacle such as the stage and smoothly flows in the film-forming container 1A. This means that the cleaning gas containing fluorine radials in an active state can be distributed to every corner portion of the film-forming container 1A without deactivating the fluorine radicals according to the cleaning method adopting the sixth feature in the second embodiment. Therefore, according to the sixth feature in the second embodiment, since the chemical reaction between the fluorine radicals in an active state and the unnecessary film formed at the corner portions of the film-forming container 1A is promoted, it is possible to sufficiently remove the unnecessary film formed at the corner portions of the film-forming container 1A.
In particular, in the cleaning method adopting the sixth feature in the second embodiment, the source gas supply port 14 functions as a cleaning gas supply port, and the source gas exhaust port 15 functions as a cleaning gas exhaust port. This means that the cleaning gas containing fluorine radicals flows through the same path as the source gas flowing in the film-forming container 1A in the cleaning method according to the second embodiment. As a result, in the cleaning method according to the second embodiment, the unnecessary film formed in correspondence with the flowing state of the source gas can be removed without fail by the cleaning gas containing fluorine radicals that flows in the film-forming container 1A through the same path as the source gas.
<Modification>
Subsequently, a modification of the second embodiment will be described.
<Consideration for Further Improvement>
For example, as shown in
<Plasma Atomic Layer Deposition Apparatus>
In
Next, features in the third embodiment will be described. The seventh feature in the third embodiment is that the source gas supply port 14a for introducing the source gas into the film-forming container 2A and the reaction gas supply port 14b for introducing the reaction gas into the film-forming container 2A are provided as separate constituent elements as shown in
Subsequently, the eighth feature in the third embodiment is that an inner dimension size of the source gas supply port 14a is larger than an inner dimension size of the reaction gas supply port 14b as shown in
<Atomic Layer Deposition Method>
The plasma atomic layer deposition apparatus 2 according to the third embodiment is configured as described above, and an atomic layer deposition method using the plasma atomic layer deposition apparatus 2 will be described below with reference to drawings.
First, as shown in
Next, as shown in
Subsequently, as shown in
Further, as shown in
In the above-described manner, it is possible to form a film in a unit of atomic layer over the substrate 10 by using the plasma atomic layer deposition apparatus 2 according to the third embodiment.
In the fourth embodiment, the technical idea in which the occurrence potential of the foreign matter in the film-forming container is reduced by removing the unnecessary film formed in the film-forming container, thereby improving the quality of the film formed over the substrate, on the premise of the configuration of the plasma atomic layer deposition apparatus 2 according to the third embodiment will be described. Specifically, in the fourth embodiment, the technique of cleaning the plasma atomic layer deposition apparatus in the third embodiment will be described.
Thus, in the fourth embodiment, the technical idea of cleaning the plasma atomic layer deposition apparatus 2 according to the third embodiment in which the unnecessary films are formed in the film-forming container 2A will be described.
As described above, in the plasma atomic layer deposition apparatus 2 according to the fourth embodiment, since the cleaning gas containing fluorine radicals is introduced from both the source gas supply port 14a and the reaction gas supply port 14b, the films 60a to 60c which are the unnecessary films formed in the film-forming container 2A shown in
<Consideration for Improvement Focused on Cost Reduction>
In the cleaning method according to the fourth embodiment, as shown in
<Cleaning Method in Fifth Embodiment>
In particular, in the cleaning method according to the fifth embodiment, the cleaning gas containing fluorine radicals is not introduced from the reaction gas supply port 14b but is introduced from the source gas supply port 14a. This is because the inner dimension size of the source gas supply port 14a is larger than the inner dimension size of the reaction gas supply port 14b and it is possible to smoothly supply the cleaning gas containing fluorine radicals into the film-forming container 2A from the source gas supply port 14a. Namely, from the viewpoint of efficiently performing the cleaning, it is important to smoothly introduce the cleaning gas containing fluorine radicals into the film-forming container 2A and to promptly exhaust the cleaning gas containing fluorine radicals from the source gas exhaust port 15.
Further, when fluorine radicals collide with an inner wall, the fluorine radicals are deactivated and become unable to demonstrate the cleaning effect. Therefore, when the cleaning gas containing fluorine radicals is introduced into the film-forming container 2A from the reaction gas supply port 14b whose inner dimension size is smaller than that of the source gas supply port 14a, the probability of collision with an inner wall of a pipe communicating with the reaction supply port 14b in the stage prior to being supplied into the film-forming container 2A increases, and the possibility that the fluorine radicals are deactivated increases. Thus, when the cleaning gas containing fluorine radicals is introduced into the film-forming container 2A from the reaction gas supply port 14b whose inner dimension size is smaller than that of the source gas supply port 14a, the efficiency of removing the necessary film adhered to the inside of the film-forming container 2A is lowered.
On the other hand, in the fifth embodiment, the cleaning gas containing fluorine radicals is introduced into the film-forming container 2A from the source gas supply port 14a whose inner dimension size is larger than that of the reaction gas supply port 14b. Thus, the probability of deactivation of the fluorine radicals is lowered, as compared with the case where the fluorine radicals are introduced into the film-forming container 2A from the reaction gas supply port 14b. Consequently, in the cleaning method according to the fifth embodiment, it is possible to suppress the reduction in the removal efficiency of the unnecessary film adhered to the inside of the film-forming container 2A, while achieving the cost reduction by reducing the flow rate of the cleaning gas containing fluorine radicals.
<Side Effect>
However, when the cleaning method according to the fifth embodiment is adopted, the following side effect occurs. The side effect will be described below.
In
The ninth feature in the fifth embodiment is that the process described below is performed together with the process in which the cleaning gas containing fluorine radicals is introduced into the film-forming container 2A from the source gas supply port 14a and the cleaning gas is exhausted to the outside of the film-forming container 2A from the source gas exhaust port 15 as shown in
<Basic Idea in Sixth Embodiment>
The basic idea in the sixth embodiment is premised on the configuration in which a plurality of supply paths for supplying the cleaning gas containing fluorine radicals into the film-forming container are provided and a plurality of exhaust paths for exhausting the cleaning gas to the outside of the film-forming container are provided. Further, the basic idea in the sixth embodiment is that the flow of the cleaning gas containing fluorine radicals in the film-forming container is controlled by switching the supply path and switching the exhaust path by a control unit provided in the plasma atomic layer deposition apparatus. According to the basic idea in the sixth embodiment described above, since the flow of the cleaning gas can be changed such that the cleaning gas can reach the place (dead space) which the cleaning gas does not reach by the single flow of the cleaning gas, it is possible to eliminate the place which the cleaning gas does not reach. This means that the unnecessary film left without being removed in the dead space is reduced by adopting the basic idea in the sixth embodiment. Thus, according to the basic idea in the sixth embodiment, it is possible to sufficiently remove the unnecessary film formed in the film-forming container. In the following, the schematic configuration of the plasma atomic layer deposition apparatus that embodies the basic idea in the sixth embodiment will be described with reference to drawings.
<Configuration of Plasma Atomic Layer Deposition Apparatus>
Further, the plasma atomic layer deposition apparatus 3 according to the sixth embodiment includes a plurality of valves 80 provided in correspondence with each of the plurality of cleaning gas ports 70 and configured to be openable and closable and a control unit 90 for controlling the open and close of each of the plurality of valves 80. At this time, the control unit 90 is configured so as to control the flow of the cleaning gas in the film-forming space 13 by controlling the open and close of each of the plurality of valves 80.
Specifically, in the cleaning method using the plasma atomic layer deposition apparatus 3 according to the sixth embodiment, the control unit 90 provided in the plasma atomic layer deposition apparatus 3 controls the open and close of each of the plurality of valves 80, thereby setting the supply path of the cleaning gas and the exhaust path of the cleaning gas. Thereafter, the plasma atomic layer deposition apparatus 3 supplies the cleaning gas into the film-forming container 3A through the supply path of the cleaning gas set by the control unit 90. Then, the plasma atomic layer deposition apparatus 3 exhausts the cleaning gas to the outside of the film-forming container 3A through the exhaust path of the cleaning gas set by the control unit 90. Thereafter, for example, after a predetermined time elapses, the open and close of each of the plurality of valves 80 are switched by the control unit 90. Thus, the flow of the cleaning gas in the film-forming container 3A can be changed by the switched supply path of the cleaning gas and the switched exhaust path of the cleaning gas. As a result, according to the cleaning method in the sixth embodiment, it is possible to eliminate the place which the cleaning gas does not reach. Therefore, according to the cleaning method using the plasma atomic layer deposition apparatus 3 in the sixth embodiment, it is possible to sufficiently remove the unnecessary film formed in the film-forming container 3A. Namely, according to the cleaning method using the plasma atomic layer deposition apparatus 3 in the sixth embodiment, it is possible to reduce the unnecessary film adhered and left without being removed in the film-forming container 3A. Consequently, according to the cleaning method using the plasma atomic layer deposition apparatus 3 in the sixth embodiment, since it is possible to suppress the foreign matter made of the peeled film from being adhered to the substrate, the quality of the film formed over the substrate can be improved.
Note that, in the sixth embodiment, the example in which the control unit 90 is provided in the plasma atomic layer deposition apparatus 3 has been described, but the basic idea in the sixth embodiment is not limited to this, and the control unit 90 may be provided outside the plasma atomic layer deposition apparatus 3.
In the foregoing, the invention made by the inventors of the present invention has been concretely described based on the embodiments. However, it is needless to say that the present invention is not limited to the foregoing embodiments and various modifications and alterations can be made within the scope of the present invention.
Number | Date | Country | Kind |
---|---|---|---|
JP2017-154942 | Aug 2017 | JP | national |
Number | Name | Date | Kind |
---|---|---|---|
6251216 | Okamura | Jun 2001 | B1 |
20030079757 | Shibata et al. | May 2003 | A1 |
20030121886 | Strang | Jul 2003 | A1 |
20050039773 | Moriya | Feb 2005 | A1 |
20060292310 | Le | Dec 2006 | A1 |
20130309401 | Miyatake | Nov 2013 | A1 |
20160086773 | Senzaki | Mar 2016 | A1 |
Number | Date | Country |
---|---|---|
2002043288 | Feb 2002 | JP |
2002-280376 | Sep 2002 | JP |
2014-210946 | Nov 2014 | JP |
Entry |
---|
English Machine Translation JP2002043288_Okamoto (Year: 2002). |
Number | Date | Country | |
---|---|---|---|
20190048463 A1 | Feb 2019 | US |