Abstract
Atomic layer deposition processes for forming germanium oxide thin films are provided. In some embodiments the ALD processes can include the following: contacting the substrate with a vapor phase tetravalent Ge precursor such that at most a molecular monolayer of the Ge precursor is formed on the substrate surface; removing excess Ge precursor and reaction by products, if any; contacting the substrate with a vapor phase oxygen precursor that reacts with the Ge precursor on the substrate surface; removing excess oxygen precursor and any gaseous by-products, and repeating the contacting and removing steps until a germanium oxide thin film of the desired thickness has been formed.
Description
BACKGROUND OF THE INVENTION
Field of the Invention

The application relates to atomic layer deposition processes for forming GeO2 films.


Background

Ge devices are of interest because of Ge high hole mobility. Low Da interface formation with HfO2 HK material will allow for good Ge based FinFETs.


SUMMARY

According to some embodiments of the present disclosure, atomic layer deposition processes for forming germanium oxide thin films on a substrate in a reaction chamber are disclosed. The ALD processes can include contacting the substrate with a vapor phase tetravalent Ge precursor, removing excess Ge precursor and any reaction by-products, contacting the substrate with a vapor phase oxygen precursor, removing excess oxygen precursor and any gaseous by-products, and repeating the contacting and removing steps until a germanium oxide thin film of the desired thickness has been formed. In some embodiments, contacting the substrate with a vapor phase tetravalent Ge precursor results in the formation of at most a molecular monolayer of the Ge precursor on the substrate surface. In some embodiments, the oxygen precursor reacts with the Ge precursor on the substrate surface.


According to some embodiments of the present disclosure, in an ALD process for forming a germanium oxide thin film using a Ge precursor and an oxygen precursor, removing excess Ge precursor comprising removing excess Ge precursor from the substrate surface and in the proximity of the substrate surface. In some embodiments, the oxygen precursor is something other than water. In some embodiments, the oxygen precursor is one of ozone, oxygen atoms, oxygen radicals, or oxygen plasma. In some embodiments, the Ge-precursor is not a halide. In some embodiments, the Ge-precursor comprises at least one alkoxide ligand. In some embodiments, the Ge-precursor comprises at least one amine or alkylamine ligand. In some embodiments, the Ge-precursor comprises at least one amine or alkylamine ligand, and the oxygen precursor comprises water.


According to some embodiments of the present disclosure, in an ALD process for forming a germanium oxide thin film on a substrate, the surface of the substrate comprises a thin layer of GeO2 prior to beginning the ALD process. In some embodiments, the substrate is pretreated with a passivation chemical to prevent oxidation before the germanium oxide film is deposited. In some embodiments, an interfacial layer is formed on the substrate before the germanium oxide thin film is deposited. In some embodiments, the deposition temperature is from about 100° C. to about 400° C. In some embodiments, the substrate is treated to remove native Ge oxide prior to forming the germanium oxide thin film.


Some embodiments for forming a germanium oxide thin film by an ALD process include depositing a thin layer of a different material over the germanium oxide thin film. In some embodiments, the thin layer of a different material is deposited directly on the germanium oxide thin film. In some embodiments, the thin layer comprises Al2O3, and in some embodiments, the Al2O3 layer is deposited by a process that does not use water as a reactant. In some embodiments, the germanium oxide thin film serves as an interlayer between the substrate and a high-k layer. And in some embodiments, the germanium oxide thin film may be used in a Ge-condensation process.


According to some embodiments, an atomic layer deposition process is disclosed for forming a pure GeO2 thin film, in which the process can include alternately and sequentially contacting a substrate with Ge(OCH2CH3)4 and O3.


According to some embodiments, an atomic layer deposition process is disclosed for forming a pure GeO2 thin film, which can include alternately and sequentially contacting a substrate with an alkylamine Ge precursor and an oxygen source. In some embodiments, the Ge precursor is TDMAGe, and the oxygen source is ozone. And in some embodiments, the Ge precursor is TDMAGe, and the oxygen source is water. In some embodiments, the oxygen source is water.





BRIEF DESCRIPTION OF THE DRAWINGS

The invention will be better understood from the Detailed Description and from the appended drawings, which are meant to illustrate and not to limit the invention, and wherein:



FIG. 1 illustrates the growth rate of GeO2 films as a function of deposition temperature using vapour pulses of Ge(OEt)4 and O3 at 150° C.-300° C.;



FIG. 2 illustrates two computerized images of the respective thicknesses of two wafers prepared according to some embodiments.



FIG. 3 illustrates GeO2 film thickness non-uniformity as a function of deposition temperature using vapour pulses of Ge(OEt)4 and O3 at 150° C.-300° C.;



FIG. 4 illustrates GeO2 film thickness as a function of the number of deposition cycles when using vapour pulses of Ge(OEt)4 and O3 at 250° C.;



FIG. 5 shows the composition of GeO2 deposited by ALD at various temperatures.



FIG. 6A shows GeO2 films deposited by ALD over Ge at a first magnification. HfO2 was subsequently deposited over the GeO2;



FIG. 6B shows GeO2 films deposited by ALD over Ge at a second magnification. HfO2 was subsequently deposited over the GeO2;



FIG. 7A illustrates GeO2 film thickness as a function of the number of deposition cycles when using vapour pulses of Ge(OEt)4 and O3 at 300° C. on HF-last Si;



FIG. 7B illustrates GeO2 film thickness as a function of the number of deposition cycles when using vapour pulses of Ge(OEt)4 and O3 at 300° C. on HF-last Ge;



FIG. 8A shows a transmission electron microscope (TEM) image of two layers deposited by ALD (GeO2 and Al2O3) where the Al2O3 was deposited using a TMA+O3-process.



FIG. 8B shows a TEM image of three intermixed layers (Al, Ge, and O) when Al2O3 was deposited using a TMA+H2O process.



FIG. 9A shows an image from a scanning electron microscope (SEM) at a first magnification illustrating GeO2 film conformality when deposited using vapour pulses of Ge(OEt)4 and O3.



FIG. 9B shows an image from a SEM at a second magnification illustrating GeO2 film conformality when deposited using vapour pulses of Ge(OEt)4 and O3.



FIG. 10 illustrates ALD GeO2/ALD HfO2 stack film conformality when grown at reaction temperature of 250° C. The target thickness of the GeO2 was about 30 nm.



FIG. 11 illustrates the C-V characteristics of ALD GeO2 interlayers grown on p-doped Ge and n-doped Ge. The GeO2 interlayers were grown at a reaction temperature 250° C. from vapour pulses of Ge(OEt)4 and O3.



FIG. 12 illustrates the C-V characteristics of GeO2 interlayer grown by ALD at different temperatures using vapour pulses of Ge(OEt)4 and O3.



FIG. 13A illustrates the C-V characteristics of GeO2 interlayers, grown by ALD at a reaction temperature of 250° C. using vapour pulses of Ge(OEt)4 and O3 with an ALD Al2O3 capping layer.



FIG. 13B illustrates the C-V characteristics of GeO2 interlayers, grown by ALD at a reaction temperature of 250° C. using vapour pulses of Ge(OEt)4 and O3 without an ALD Al2O3 capping layer.



FIG. 14A illustrates the C-V characteristics of GeO2 interlayers grown by ALD on Ge-substrates with HF-cleaning, at a reaction temperature 250° C. using vapour pulses of Ge(OEt)4 and O3.



FIG. 14B illustrates the C-V characteristics of GeO2 interlayers grown by ALD on Ge-substrates without HF-cleaning, at a reaction temperature 250° C. using vapour pulses of Ge(OEt)4 and O3.





DETAILED DESCRIPTION

In one aspect, methods of depositing GeO2 thin films by atomic layer deposition are provided. In some embodiments a GeO2 thin film is formed on a substrate by a vapor deposition process comprising alternately and sequentially contacting a substrate with a vapor phase germanium precursor and an oxygen reactant, such that a layer of the germanium precursor forms on the substrate surface, and the oxygen-containing reactant subsequently reacts with the germanium precursor to form a GeO2 thin film.


In some embodiments the Ge precursor may be selected from Germanium ethoxide (GeOEt)4 and tetrakis(dimethylamino) germanium (TDMAGe). Other possible germanium precursors are provided below. In some embodiments the Ge precursor is not a halide. In some embodiments, the Ge precursor contains halide in at least one ligand, but not in all ligands.


In some embodiments the oxygen reactant comprises one or more of ozone, oxygen atoms, oxygen radicals, and oxygen plasma. In some embodiments the oxygen reactant may be water. However, in other embodiments the oxygen reactant is not water.


In some embodiments, GeO2 thin films are deposited by alternately and sequentially contacting a substrate with Ge(OCH2CH3)4 and O3. In some embodiments GeO2 thin films are deposited by alternately and sequentially contacting a substrate with tetrakis(dimethylamio) germanium (TDMAGe) and O3.


GeO2 films may be used, for example as an interface layer between high-k and new channel materials in semiconductor devices. For example, the GeO2 layer may serve as an interface in a Ge-based FinFET. In some embodiments the GeO2 layer is an interface layer between Ge and a high-k material. The GeO2 interface layer may prevent leakage and decrease trap density. Other contexts in which GeO2 thin films may be utilized will be apparent to the skilled artisan. For example, GeO2 thin films may find use in optical applications. In some embodiments, the GeO2 films deposited by ALD processes are annealed after the deposition as desired depending on the application.


In one embodiment, the GeO2 films deposited by ALD can be used for a process called Ge-condensation. A principle of this can be seen and understood, for example, from U.S. Patent Publications 2011/0147811 (see FIGS. 3a and 3b) and 2011/0193178 (see para. [0020, which are incorporated by reference herein]). By adding a GeO2 film to the interface of Si1-xGexSiO2, it may be possible for more Ge to be driven to the fin or channel material. In these cases it is preferable to cap the ALD-deposited GeO2 film with another film (i.e., a “capping layer”), preferably one deposited by ALD or PEALD, such as ALD-deposited or PEALD-deposited Al2O3, SiNx, or SiO2 before an anneal step where Ge will be driven to the fin or channel. In this application of Ge-condensation, water may be used as an oxygen source in the ALD GeO2 process. In some embodiments, the GeO2 is deposited by an ALD process on a silicon fin without further depositing a capping layer. In some embodiments, the GeO2 is deposited by an ALD process on a Si1-xGex fin without further depositing a capping layer. In some embodiments, the GeO2 is deposited by an ALD process on a silicon fin and a capping layer is deposited over the GeO2 layer. In some embodiments, the GeO2 is deposited by an ALD process on a Si1-xGex fin, and a capping layer is then deposited over the GeO2 layer. In some embodiments, the capping layer is SiO2. In some embodiments, the capping layer is SiNx. In some embodiments, the capping layer is Al2O3. In some embodiments, the capping layer is deposited by methods other than an ALD or PEALD process. In some embodiments, the capping layer is deposited by an ALD process. In some embodiments the capping layer is deposited by a PEALD process.


In some embodiments the GeO2 films deposited by ALD are pure GeO2 films. Thus, deposited GeO2 may be able to produce a better interface layer than GeO2 formed by thermal oxidation.


Atomic layer deposition allows for conformal deposition of GeO2 films. In some embodiments, the GeO2 films deposited by ALD have at least 90%, 95% or higher conformality. In some embodiments the films are about 100% conformal.


The substrate may be, for example, a semiconductor substrate. In some embodiments the surface of the substrate comprises a group III or group IV compound. For example, in some embodiments the surface of the substrate comprises Ge. In some embodiments the surface of the substrate comprises a thin GeO2 layer. The GeO2 layer may be formed, for example, through thermal or plasma oxidation. In some embodiments the substrate surface is H-terminated. In some embodiments native Ge oxide is removed, for example with HF, prior to GeO2 deposition by ALD.


The substrate may be treated prior to depositing the GeO2 layer by ALD. For example, the substrate may be treated with a passivation chemical to prevent oxidation prior to depositing GeO2 by ALD. In other embodiments the substrate is treated to form an interfacial layer prior to depositing GeO2 by ALD. For example, the substrate treatment may comprise exposing the substrate to trimethylaluminum (TMA) to form an interfacial layer or surface termination on the surface prior to GeO2 deposition. As mentioned above, in some embodiments the substrate may be treated to remove native Ge oxide, for example with HF, prior to depositing GeO2 by ALD.


In some embodiments, following GeO2 deposition, a further film is deposited. The additional film may be directly over and contacting the ALD-deposited GeO2 layer. In some embodiments a high-k film is deposited after the ALD-deposited GeO2 is deposited. The high-k layer or other film may be deposited by ALD or by other known deposition methods. In some embodiments a HfO2 layer is deposited over the GeO2 layer. In some embodiments an Al2O3 layer is deposited over the GeO2 layer. Without being bound to any particular theory, it is believed that water in the deposition process of the layer deposited on top of a GeO2 layer may cause in some situations the intermixing of the already deposited GeO2 layer and the layer deposited on top of GeO2 layer. In some embodiments this mixing is preferable. In other embodiments, this mixing is to be avoided. Thus, in some embodiments a deposition process for depositing a film on top of a GeO2 film does not utilize water as one of the reactants. In some embodiments a deposition process for depositing a film on top of a GeO2 film utilizes an oxygen source other than water. In some embodiments, a deposition process for a film deposited on top of a GeO2 film uses ozone as an oxygen source. In some embodiments a deposition process for a film deposited on top of a GeO2 film uses oxygen atoms, oxygen radicals or oxygen containing plasma as an oxygen source. In some embodiments, a deposition process for a film deposited on top of a GeO2 film uses water, and at least one mixed layer comprising germanium is produced. When a Ge substrate is used and ozone or oxygen plasma are provided as an oxygen source, atoms or radicals may oxidize the substrate during the first one or more ALD cycles for forming GeO2 and form a thin layer of GeO2 on the substrate itself. In that situation, the GeO2 layer would be a kind of composite of GeO2 (oxidized from substrate) and ALD-deposited GeO2.


In some embodiments a GeO2 layer is an interlayer between a substrate and high-k layer. Preferably a GeO2 interlayer has a thickness of less than about 10 nm, more preferably less than about 5 nm and most preferably less than about 3 nm. In some cases the GeO2 interlayer is less than about 2 nm or even less than about 1 nm thick.


Atomic Layer Deposition (ALD)


As noted above, processes described herein enable use of atomic layer deposition techniques to deposit conformal GeO2 layers. Among vapor deposition techniques, ALD has the advantage of providing high conformality at low temperatures.


ALD type processes are based on controlled, self-limiting surface reactions of precursor chemicals. Gas phase reactions are avoided by feeding the precursors alternately and sequentially into the reaction chamber. Vapor phase reactants are separated from each other in the reaction chamber, for example, by removing excess reactants and/or reactant by-products from the reaction chamber between reactant pulses.


Briefly, a substrate is loaded into a reaction chamber and is heated to a suitable deposition temperature, generally at lowered pressure. Deposition temperatures are maintained below the precursor thermal decomposition temperature but at a high enough level to avoid condensation of reactants and to provide the activation energy for the desired surface reactions. Of course, the appropriate temperature window for any given ALD reaction will depend upon the surface termination and reactant species involved. In some embodiments the deposition temperature is from about 20° C. to about 600° C., preferably from about to 100° C. to about 400° C., and more preferably from about 150° C. to about 300° C.


A first germanium reactant is conducted into the chamber in the form of vapor phase pulse and contacted with the surface of a substrate. In some embodiments the substrate surface comprises a three dimensional structure. Conditions are preferably selected such that no more than about one monolayer of the germanium precursor is adsorbed on the substrate surface in a self-limiting manner. Excess first reactant and reaction byproducts, if any, may be removed from the substrate and substrate surface and from proximity to the substrate and substrate surface. In some embodiments reactant and reaction byproducts, if any, may be removed by purging. Purging may be accomplished for example, with a pulse of inert gas such as nitrogen or argon.


Purging the reaction chamber means that vapor phase precursors and/or vapor phase byproducts are removed from the reaction chamber such as by evacuating the chamber with a vacuum pump and/or by replacing the gas inside the reactor with an inert gas such as argon or nitrogen. Typical purging times are from about 0.05 seconds to about 20 seconds, more preferably between about 1 second and about 10 seconds, and still more preferably between about 1 second and about 2 seconds. However, other purge times can be utilized if necessary, such as when depositing layers over extremely high aspect ratio structures or other structures with complex surface morphology. The appropriate pulsing times can be readily determined by the skilled artisan based on the particular circumstances.


Another method for removing excess reactants—metal precursors or oxygen precursors, reaction byproducts, etc.—from the substrate surface or from the area of the substrate may involve physically moving the substrate from a location containing the reactant and/or reaction byproducts.


A second gaseous oxygen reactant is pulsed into the chamber where it reacts with the first germanium reactant on the surface to form germanium oxide. Excess second reactant and gaseous by-products of the surface reaction are removed from the substrate, for example by purging them out of the reaction chamber, preferably with the aid of an inert gas. The steps of pulsing and removing are repeated until a thin film of the desired thickness has been formed on the substrate, with each cycle typically leaving no more than about a molecular monolayer.


As mentioned above, each pulse or phase of each cycle is preferably self-limiting. An excess of reactant precursors is supplied in each phase to saturate the susceptible structure surfaces. Surface saturation ensures reactant occupation of all available reactive sites (subject, for example, to physical size or “steric hindrance” restraints) and thus ensures excellent step coverage. In some arrangements, the degree of self-limiting behavior can be adjusted by, e.g., allowing some overlap of reactant pulses to trade off deposition speed (by allowing some CVD-type reactions) against conformality. Ideal ALD conditions with reactants well separated in time and space provide near perfect self-limiting behavior and thus maximum conformality, but steric hindrance results in less than one molecular layer per cycle. Limited CVD reactions mixed with the self-limiting ALD reactions can raise the deposition speed.


In some embodiments, a reaction space can be in a single-wafer ALD reactor or a batch ALD reactor where deposition on multiple substrates takes place at the same time. In some embodiments the substrate on which deposition is desired, such as a semiconductor workpiece, is loaded into a reactor. The reactor may be part of a cluster tool in which a variety of different processes in the formation of an integrated circuit are carried out. In some embodiments a flow-type reactor is utilized. In some embodiments a high-volume manufacturing-capable single wafer ALD reactor is used. In other embodiments a batch reactor comprising multiple substrates is used. For embodiments in which batch ALD reactors are used, the number of substrates is preferably in the range of 10 to 200, more preferably in the range of 50 to 150, and most preferably in the range of 100 to 130.


Examples of suitable reactors that may be used include commercially available ALD equipment such as the F-120® reactor, F-450 reactor, Pulsar® reactors—such as the Pulsar® 2000 and the Pulsar® 3000—EmerALD® reactor and Advance® 400 Series reactors, available from ASM America, Inc of Phoenix, Ariz. and ASM Europe B.V., Almere, Netherlands. Other commercially available reactors include those from ASM Japan K.K (Tokyo, Japan) under the tradename Eagle® XP and XP8. In addition to these ALD reactors, many other kinds of reactors capable of ALD growth of thin films, including CVD reactors equipped with appropriate equipment and means for pulsing the precursors can be employed. In some embodiments a flow type ALD reactor is used. Preferably, reactants are kept separate until reaching the reaction chamber, such that shared lines for the precursors are minimized. However, other arrangements are possible.


Suitable batch reactors include, but are not limited to, reactors designed specifically to enhance ALD processes, which are commercially available from and ASM Europe B.V (Almere, Netherlands) under the trade names ALDA400™ and A412™. In some embodiments a vertical batch reactor is utilized in which the boat rotates during processing, such as the A412™. Thus, in some embodiments the wafers rotate during processing. In some embodiments in which a batch reactor is used, wafer-to-wafer uniformity is less than 3% (1 sigma), less than 2%, less than 1% or even less than 0.5%.


The germanium oxide ALD processes described herein can optionally be carried out in a reactor or reaction space connected to a cluster tool. In a cluster tool, because each reaction space is dedicated to one type of process, the temperature of the reaction space in each module can be kept constant, which improves the throughput compared to a reactor in which the substrate is heated up to the process temperature before each run.


According to some embodiments, a germanium oxide thin film is formed by an ALD-type process comprising multiple pulsing cycles, each cycle comprising:

    • pulsing a vaporized first Ge precursor into the reaction chamber to form at most a molecular monolayer of the Ge precursor on the substrate,
    • removing excess Ge precursor and reaction by products, if any,
    • providing a pulse of a second oxygen reactant comprising an oxygen source onto the substrate,
    • removing excess second reactant and any gaseous by-products formed in the reaction between the Ge precursor layer on the first surface of the substrate and the second reactant, and
    • repeating the pulsing and removing steps until a germanium oxide thin film of the desired thickness has been formed.


In some embodiments germanium oxide, preferably GeO2, is deposited from alternating and sequential pulses of a Ge precursor and an oxygen source, like water, ozone, oxygen plasma, oxygen radicals, or oxygen atoms. In some embodiments the oxygen source is not water. The Ge precursor preferably comprises Ge(OEt)4 or TDMAGe.


The Ge precursor employed in the ALD type processes may be solid, liquid, or gaseous material under standard conditions (room temperature and atmospheric pressure), provided that the Ge precursor is in vapor phase before it is conducted into the reaction chamber and contacted with the substrate surface. “Pulsing” a vaporized precursor onto the substrate means that the precursor vapor is conducted into the chamber for a limited period of time. Typically, the pulsing time is from about 0.05 seconds to about 10 seconds. However, depending on the substrate type and its surface area, the pulsing time may be even higher than about 10 seconds.


Preferably, for a 300 mm wafer in a single wafer ALD reactor, the Ge precursor is pulsed for from about 0.05 seconds to about 10 seconds, more preferably for from about 0.1 seconds to about 5 seconds and most preferably for from about 0.3 seconds to about 3.0 seconds. The oxygen-containing precursor is preferably pulsed for from about 0.05 seconds to about 10 seconds, more preferably for from about 0.1 seconds to about 5 seconds, most preferably for from about 0.2 seconds to about 3.0 seconds. However, pulsing times can be on the order of minutes in some cases. The optimum pulsing time can be readily determined by the skilled artisan based on the particular circumstances.


As mentioned above, in some embodiments the Ge precursor is Ge(OEt)4 or TDMAGe. Other possible germanium precursors that can be used in some embodiments are described below. In some embodiments, the Ge precursor is Ge(OMe)4. In some embodiments the Ge-precursor is not a halide. In some embodiments the Ge-precursor may comprise a halogen in at least one ligand, but not in all ligands.


The oxygen source may be an oxygen-containing gas pulse and can be a mixture of oxygen and inactive gas, such as nitrogen or argon. In some embodiments the oxygen source may be a molecular oxygen-containing gas pulse. The preferred oxygen content of the oxygen-source gas is from about 10% to about 25%. Thus, one source of oxygen may be air. In some embodiments, the oxygen source is molecular oxygen. In some embodiments, the oxygen source comprises an activated or excited oxygen species. In some embodiments, the oxygen source comprises ozone. The oxygen source may be pure ozone or a mixture of ozone, molecular oxygen, and another gas, for example an inactive gas such as nitrogen or argon. Ozone can be produced by an ozone generator and it is most preferably introduced into the reaction space with the aid of an inert gas of some kind, such as nitrogen, or with the aid of oxygen. In some embodiments, ozone is provided at a concentration from about 5 vol-% to about 40 vol-%, and preferably from about 15 vol-% to about 25 vol-%. In other embodiments, the oxygen source is oxygen plasma.


In some embodiments, ozone or a mixture of ozone and another gas is pulsed into the reaction chamber. In other embodiments, ozone is formed inside the reactor, for example by conducting oxygen containing gas through an arc. In other embodiments, an oxygen containing plasma is formed in the reactor. In some embodiments, the plasma may be formed in situ on top of the substrate or in close proximity to the substrate. In other embodiments, the plasma is formed upstream of the reaction chamber in a remote plasma generator and plasma products are directed to the reaction chamber to contact the substrate. As will be appreciated by the skilled artisan, in the case of a remote plasma, the pathway to the substrate can be optimized to maximize electrically neutral species and minimize ion survival before reaching the substrate.


In some embodiments the oxygen source is an oxygen source other than water. Thus, in some embodiments water is not provided in any ALD cycle for depositing GeO2.


In some embodiments the Ge precursor comprises at least one amine or alkylamine ligand, such as those presented in formulas (2) through (6) and (8) and (9), and the oxygen precursor comprises water.


Before starting the deposition of the film, the substrate is typically heated to a suitable growth temperature, as discussed above. The preferred deposition temperature may vary depending on a number of factors such as, and without limitation, the reactant precursors, the pressure, flow rate, the arrangement of the reactor, and the composition of the substrate including the nature of the material to be deposited on.


The processing time depends on the thickness of the layer to be produced and the growth rate of the film. In ALD, the growth rate of a thin film is determined as thickness increase per one cycle. One cycle consists of the pulsing and removing steps of the precursors and the duration of one cycle is typically between about 0.2 seconds and about 30 seconds, more preferably between about 1 second and about 10 seconds, but it can be on order of minutes or more in some cases, for example, where large surface areas and volumes are present.


In some embodiments the GeO2 film formed is a pure GeO2 film. Preferably, aside from minor impurities no other metal or semi-metal elements are present in the film. In some embodiments the film comprises less than 1-at % of metal or semi-metal other than Ge. In some embodiments the GeO2 film is stoichiometric. In some embodiments, a pure GeO2 film comprises less than about 5-at % of any impurity other than hydrogen, preferably less than about 3-at % of any impurity other than hydrogen, and more preferably less than about 1-at % of any impurity other than hydrogen.


In some embodiments, the GeO2 film formed has step coverage of more than about 80%, more preferably more than about 90%, and most preferably more than about 95% in structures which have high aspect ratios. In some embodiments high aspect ratio structures have an aspect ratio that is more than about 3:1 when comparing the depth or height to the width of the feature. In some embodiments the structures have an aspect ratio of more than about 5:1, or even an aspect ratio of 10:1 or greater.


Ge Precursors


A number of different Ge precursors can be used in the ALD processes. In some embodiments the Ge precursor is tetravalent (i.e. Ge has an oxidation state of +IV). In some embodiments, the Ge precursor is not divalent (i.e., Ge has an oxidation state of +II). In some embodiments, the Ge precursor may comprise at least one alkoxide ligand. In some embodiments, the Ge precursor may comprise at least one amine or alkylamine ligand. In some embodiments the Ge precursor is a metal-organic or organometallic compound. In some embodiments the Ge precursor comprises at least one halide ligand. In some embodiments the Ge precursor does not comprise a halide ligand.


In some embodiments the Ge precursor is not solid at room temperature (e.g., about 20° C.).


For example, Ge precursors from formulas (1) through (9) below may be used in some embodiments.

GeOR4  (1)


Wherein R is can be independently selected from the group consisting of alkyl and substituted alkyl;

GeRxA4-x  (2)


Wherein the x is an integer from 1 to 4;


R is an organic ligand and can be independently selected from the group consisting of alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines; and


A can be independently selected from the group consisting of alkyl, substituted alkyl, alkoxides, alkylsilyls, alkyl, alkylamines, halide, and hydrogen.

Ge(OR)xA1-x  (3)


Wherein the x is an integer from 1 to 4;


R can be independently selected from the group consisting of alkyl and substituted alkyl; and


A can be independently selected from the group consisting of alkyl, alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines, halide, and hydrogen.

Ge(NRIRII)4  (4)


Wherein RI can be independently selected from the group consisting of hydrogen, alkyl and substituted alkyl; and


RII can be independently selected from the group consisting of alkyl and substituted alkyl;

Ge(NRIRII)xA1-x  (5)


Wherein the x is an integer from 1 to 4;


RI can be independently selected from the group consisting of hydrogen, alkyl and substituted alkyl; and


RII can be independently selected from the group consisting of alkyl and substituted alkyl;


A can be independently selected from the group consisting of alkyl, alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines, halide, and hydrogen.

Gen(NRIRII)2n+2  (6)


Wherein the n is an integer from 1 to 3;


RI can be independently selected from the group consisting of hydrogen, alkyl and substituted alkyl; and


RII can be independently selected from the group consisting of alkyl and substituted alkyl;

Gen(OR)2n+2  (7)


Wherein the n is an integer from 1 to 3; and


Wherein R can be independently selected from the group consisting of alkyl and substituted alkyl;

GenR2n−2  (8)


Wherein the n is an integer from 1 to 3; and


R is an organic ligand and can be independently selected from the group consisting of alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines.

A3-xRxGe-GeRyA3-y  (9)


Wherein the x is an integer from 1 to 3;


y is an integer from 1 to 3;


R is an organic ligand and can be independently selected from the group consisting of alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines; and


A can be independently selected from the group consisting of alkyl, alkoxides, alkylsilyls, alkyl, substituted alkyl, alkylamines, halide, and hydrogen.


Preferred options for R include, but are not limited to, methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tertbutyl for all formulas, more preferred in ethyl and methyl. In some embodiments, the preferred options for R include, but are not limited to, C3-C10 alkyls, alkenyls, and alkynyls and substituted versions of those, more preferably C3-C6 alkyls, alkenyls, and alkenyls and substituted versions of those.


In some embodiments the Ge precursor comprises one or more halides. Preferably the precursor comprises 1, 2, or 3 halide ligands. However, as mentioned above, in some embodiments the Ge precursor used in the ALD process does not comprise a halide.


In some embodiments, a Ge precursor that comprises an alkoxide is not used in combination with water in an ALD process. In other embodiments, an amine/akylyamine or Ge-N bond containing Ge precursor may be used in combination with water. Preferred alkylamine Ge precursors include, but are not limited to, tetrakis(dimethylamino) germanium (TDMAGe), tetrakis(diethylamino) germanium (TDEAGe), and tetrakis(ethylmethylamino) germanium (TEMAGe). In some embodiments the Ge precursor is TDMAGe. In some embodiments the precursor is TDEAGe. In some embodiments the precursor is TEMAGe.


Examples

GeO2 films were deposited in an F-450 ALCVD R&D reactor at temperatures ranging from about 150° C. to about 300° C. using germanium ethoxide (Ge(OEt)4) or tetrakis(dimethylamino) germanium (TDMAGe) as the Ge precursor, and ozone (O3) as the oxygen source. Ge(OEt)4 is a liquid with a vapor pressure of about 0.2 Torr at 55° C. TDMAGe is a liquid with a vapor pressure of about 3 Torr at 50° C. Pulse/purge times were 3.0 s/6.0 s for all precursors Ge(OEt)4, TDMAGe and O3. In these deposition experiments the Ge precursor was held at room temperature. The O3 flow rate was 100 sccm. Film thicknesses were measured using a spectroscopic ellipsometer and x-ray diffraction XRR (Bruker AXS D8 Advance). Composition was determined by Rurherford backscattering spectroscopy RBS.


In one set of experiments, GeO2 films were deposited by alternately and sequentially contacting a substrate in a reactor chamber with vapor pulses of Ge(OEt)4 and O3 at about 150° C. to about 300° C. In this temperature range growth rate of about 0.18 Å/cycle to about 0.3 Å/cycle was obtained (FIG. 1).


In the same temperature range of 150° C. to 300° C. the thickness non-uniformity was about 3% to about 13% 1-sigma, and the lowest non-uniformities were obtained at 300° C. (FIG. 3). A series of films of various thicknesses were deposited at 250° C. by varying cycle number. Film growth was linear, i.e. film thickness can be controlled by the number of cycles (FIG. 4). Thinner films were also deposited at 300° C. Between about 150° C. and about 300° C., the GeO2 film density was about 3.8 g/cm3 to about 4 g/cm3 (from XRR; bulk 4.23 g/cm3). In particular, at 250° C. the growth rate was about 0.25 Å/cycle and the film had a non-uniformity of less than about 10%. The XRR density at 250° C. was about 4.35 g/cm3 (bulk 4.23 g/cm3), and the refractive index was modeled to be close to the bulk value from ellipsometer data (bulk 1.650 vs. modeled 1.66).


In the temperature range of 150° C. to 250° C., the composition of these films was about 32-at % Ge and about 68-at % O (RBS analysis of about 50 nm GeO2 on silicon with native oxide). See FIG. 5.


Electrical results (capacitance-voltage i.e. C-V) of GeO2 films deposited by ALD on Ge-substrates (both n- and p-type) using vapor pulses of Ge(OEt)4 and O3 can be seen in FIG. 11 through FIG. 14B. In some samples, GeO2 ALD deposition was followed by Al2O3 ALD film deposition using TMA as aluminum source and ozone or water as oxygen source. It can be concluded from the electrical results that a GeO2 interlayer deposited by ALD provides good electrical properties including low Dit (interfacial traps) and Dbt (border traps), as well as small CV hysteresis for capacitors on p-Ge. Promising performance can thus be expected for transistors. No electrical degradation was found when ALD-deposited GeO2 interlayer thickness was reduced from about 5 nm to about 2.2 nm. It also can be concluded that the k value of ALD-deposited GeO2 is about 5.7. An ALD-deposited Al2O3 capping layer is preferable in some situations. Native Ge oxide can also be removed prior to the GeO2 ALD deposition. Better performance was also observed for ALD-deposited GeO2 interlayers grown at 250° C. compared to 300° C.


In FIGS. 7A and 7B it can be seen that GeO2 deposited by ALD grows linearly on HF-last Ge (FIG. 7B) and on HF-last Si (FIG. 7A) when using vapor pulses of Ge(OEt)4 and O3 at 300° C.



FIGS. 8A and 8B show TEM images of an ALD Al2O3/ALD GeO2 (37 cycles)/Ge/Si-stack/structure. Al2O3 was deposited by ALD using vapor pulses or TMA and water or ozone. As can been seen from FIG. 8B, layers can mix when using water as an oxygen source in the Al2O3 ALD process, whereas when using ozone as the oxygen source in the Al2O3 ALD process, two clearly separated layers can be seen in FIG. 8A. However, the reason for intermixing of the layers is unsure, and it may be caused by the electron beam in the analysis.


Good conformality can be obtained when depositing GeO2 by ALD using vapor pulses of Ge(OEt)4 and O3 as can be seen in FIGS. 9A and 9B and in FIG. 10, which illustrates ALD GeO2/ALD HfO2 stack film conformality when grown at a reaction temperature of 250° C. and using a target GeO2 thickness of about 30 nm.


In another set of experiments, GeO2 films were deposited by alternately and sequentially contacting a substrate in a reactor chamber with vapor pulses of tetrakis(dimethylamino)germanium (TDMAGe) and O3 at 150° C. to 300° C. In this temperature range growth rate of about 0.4 Å/cycle to about 0.55 Å/cycle was obtained. In the same temperature range of 150° C. to 300° C., the thickness non-uniformity was less than about 6%. The best nonuniformity of less than about 2% was observed at about 200° C. In the 150° C. to 300° C. range, the GeO2 film density was about 3.8 g/cm3 to about 4 g/cm3 (from XRR). The EDX composition was about 30 at. % Ge and about 70 at. % O. TDMAGe was also observed to react with water.


GeO2 was also deposited on a Ge surface and topped with HfO2. Briefly, 50 nm of GeO2 was deposited from TDMAGe and O3 by ALD, as described herein, on a substrate comprising either 15 nm or 1 μm Ge on Si. Subsequently, approximately 50 nm of HfO2 was deposited over the GeO2 by atomic layer deposition using alternating and sequential pulses of HfCl4 and H2O. The deposition temperature was 300° C. No etching was observed. The results are shown in FIGS. 6A and 6B.


Although certain embodiments and examples have been discussed, it will be understood by those skilled in the art that the scope of the claims extend beyond the specifically disclosed embodiments to other alternative embodiments and/or uses and obvious modifications and equivalents thereof.

Claims
  • 1. A deposition process for forming a thin film comprising germanium oxide and less than 5-at % of metal other than germanium on a substrate by multiple sequential deposition cycles, each of the sequential deposition cycles comprising: contacting the substrate with a vapor phase tetravalent germanium precursor comprising at least one ligand selected from alkyl, alkoxide, amine, and alkylamine, such that a molecular monolayer comprising germanium is formed on the substrate surface,contacting the substrate with a vapor phase oxygen precursor, wherein the oxygen precursor reacts with the monolayer comprising germanium on the substrate surface.
  • 2. The process of claim 1, each of the multiple deposition cycles further comprising removing excess germanium precursor and reaction byproducts, if any, from the substrate surface prior to contacting the substrate with the vapor phase oxygen precursor.
  • 3. The process of claim 1, each of the multiple deposition cycles further comprising removing excess oxygen precursor and reaction byproducts, if any, from the substrate surface prior to beginning a subsequent deposition cycle.
  • 4. The process of claim 1, wherein the multiple sequential deposition cycles include only a germanium precursor and an oxygen precursor.
  • 5. The process of claim 1, wherein the oxygen precursor comprises ozone, oxygen atoms, oxygen radicals, or oxygen plasma.
  • 6. The process of claim 1, wherein the germanium precursor comprises an alkylamine ligand and the oxygen precursor comprises water.
  • 7. The process of claim 6, wherein the germanium precursor has a formula Gen(NRIRII)2n+2 and RI and RII can be independently selected from methyl and ethyl.
  • 8. The process of claim 6, wherein the germanium precursor has a formula Gen(NRIRII)2n+2 and RI and RII can be independently selected from C3, C4, C5, and C6 alkyls.
  • 9. The process of claim 1, wherein the surface of the substrate comprises germanium oxide prior to beginning the deposition process.
  • 10. The process of claim 1, wherein the substrate is pretreated before the thin film is formed.
  • 11. The process of claim 10, wherein the pretreatment comprises exposing the substrate to a passivation chemical.
  • 12. The process of claim 10, wherein the pretreatment comprises forming an interfacial layer on the substrate surface.
  • 13. The process of claim 10, wherein the pretreatment comprises removing native Ge oxide from the substrate surface.
  • 14. The process of claim 1, further comprising depositing a layer comprising a different material over the thin film.
  • 15. The process of claim 14, wherein the different material comprises a high-k material.
  • 16. The process of claim 1, wherein the thin film is used in a Ge-condensation process.
  • 17. An atomic layer deposition (ALD) process for forming a thin film comprising germanium oxide and less than 5-at % of metal other than germanium, the process comprising at least two sequential deposition cycles, each of the at least two sequential deposition cycles comprising: alternately and sequentially contacting a substrate with a germanium precursor comprising at least one alkyl, alkoxide, amine, or alkylamine ligand and an oxygen source, wherein the germanium precursor is not divalent.
  • 18. The process of claim 17, wherein the germanium precursor comprises Ge(OCH2CH3)4 and the oxygen source comprises O3.
  • 19. The process of claim 17, wherein the germanium precursor comprises TDMAGe, and the oxygen source comprises ozone.
  • 20. The process of claim 17, wherein the germanium precursor comprise TDMAGe, and the oxygen source comprises water.
CROSS-REFERENCE TO RELATED APPLICATIONS

This application is a continuation of U.S. application Ser. No. 14/867,833, filed Sep. 28, 2015, which is a continuation of U.S. patent application Ser. No. 13/802,393, filed Mar. 13, 2013, now U.S. Pat. No. 9,171,715, which claims priority to U.S. Provisional Application No. 61/697,007, filed Sep. 5, 2012, and U.S. Provisional Application No. 61/713,082, filed Oct. 12, 2012, each of which is incorporated by reference in its entirety.

US Referenced Citations (160)
Number Name Date Kind
4363828 Brodsky et al. Dec 1982 A
5221413 Brasen et al. Jun 1993 A
5221556 Hawkins et al. Jun 1993 A
5256550 Laderman et al. Oct 1993 A
5259918 Akbar et al. Nov 1993 A
5308788 Fitch et al. May 1994 A
5442205 Brasen et al. Aug 1995 A
5445897 Satoh et al. Aug 1995 A
5633516 Mishima et al. May 1997 A
5766999 Sato et al. Jun 1998 A
5847409 Nakayama Dec 1998 A
5879970 Shiota et al. Mar 1999 A
5891769 Liaw et al. Apr 1999 A
6030894 Hada et al. Feb 2000 A
6093252 Wengert et al. Jul 2000 A
6107653 Fitzgerald Aug 2000 A
6154475 Soref et al. Nov 2000 A
6235568 Murthy et al. May 2001 B1
6319782 Nakabayashi Nov 2001 B1
6346732 Mizushima et al. Feb 2002 B1
6350993 Chu et al. Feb 2002 B1
6373112 Murthy et al. Apr 2002 B1
6395621 Mizushima et al. May 2002 B1
6411548 Sakui et al. Jun 2002 B1
6425951 Chu et al. Jul 2002 B1
6429098 Bensahel et al. Aug 2002 B1
6455871 Shim et al. Sep 2002 B1
6461945 Yu Oct 2002 B1
6464780 Mantl et al. Oct 2002 B1
6475865 Yang et al. Nov 2002 B1
6482705 Yu Nov 2002 B1
6525338 Mizushima et al. Feb 2003 B2
6537370 Hernandez et al. Mar 2003 B1
6555839 Fitzgerald Apr 2003 B2
6562736 Yanagawa et al. May 2003 B2
6573126 Cheng et al. Jun 2003 B2
6592942 Van Wijck Jul 2003 B1
6620743 Pagliaro, Jr. et al. Sep 2003 B2
6633066 Bae et al. Oct 2003 B1
6635110 Luan et al. Oct 2003 B1
6645836 Kanzawa et al. Nov 2003 B2
6649980 Noguchi Nov 2003 B2
6713326 Cheng et al. Mar 2004 B2
6723622 Murthy et al. Apr 2004 B2
6749687 Ferro et al. Jun 2004 B1
6770134 Maydan et al. Aug 2004 B2
6812495 Wada et al. Nov 2004 B2
6821825 Todd Nov 2004 B2
6830964 Mears et al. Dec 2004 B1
6833294 Mears et al. Dec 2004 B1
6844213 Sparks Jan 2005 B2
6855649 Christiansen et al. Feb 2005 B2
6858502 Chu et al. Feb 2005 B2
6864520 Fischetti et al. Mar 2005 B2
6875279 Chu et al. Apr 2005 B2
6887773 Gunn, III May 2005 B2
6900115 Todd May 2005 B2
6905972 Oda Jun 2005 B2
6953736 Ghyselen et al. Oct 2005 B2
6958253 Todd Oct 2005 B2
6960537 Shero et al. Nov 2005 B2
6995076 Wang et al. Feb 2006 B2
7022593 Arena et al. Apr 2006 B2
7026219 Pomarede et al. Apr 2006 B2
7037856 Maa et al. May 2006 B1
7049627 Vineis et al. May 2006 B2
7108748 Brabant et al. Sep 2006 B2
7115521 Brabant et al. Oct 2006 B2
7132338 Samoilov et al. Nov 2006 B2
7232487 Silver et al. Jun 2007 B2
7238595 Brabant et al. Jul 2007 B2
7312165 Jursich et al. Dec 2007 B2
7329593 Bauer et al. Feb 2008 B2
7357838 Lin et al. Apr 2008 B2
7387953 Figuet Jun 2008 B2
7390725 Maa et al. Jun 2008 B2
7402504 Brabant et al. Jul 2008 B2
7452757 Werkhoven et al. Nov 2008 B2
7479443 Bauer Jan 2009 B2
7608526 Cody et al. Oct 2009 B2
7682947 Brabant et al. Mar 2010 B2
7772127 Figuet et al. Aug 2010 B2
7785995 Cody et al. Aug 2010 B2
7825401 Cody et al. Nov 2010 B2
7901968 Weeks et al. Mar 2011 B2
8454928 Dussarrat Jun 2013 B2
8623734 Chen et al. Jan 2014 B2
20020034864 Mizushima et al. Mar 2002 A1
20020173104 Chang Nov 2002 A1
20020173130 Pomerede et al. Nov 2002 A1
20030036268 Brabant et al. Feb 2003 A1
20030045063 Oda Mar 2003 A1
20030080394 Babcock et al. May 2003 A1
20030082300 Todd et al. May 2003 A1
20030124818 Luo et al. Jul 2003 A1
20030139000 Bedell et al. Jul 2003 A1
20030143783 Maa et al. Jul 2003 A1
20030153161 Chu et al. Aug 2003 A1
20030157787 Murthy et al. Aug 2003 A1
20030162348 Yeo et al. Aug 2003 A1
20030190791 Fischetti et al. Oct 2003 A1
20030207127 Murthy et al. Nov 2003 A1
20030230233 Fitzgerald et al. Dec 2003 A1
20030235931 Wada et al. Dec 2003 A1
20040075105 Leitz et al. Apr 2004 A1
20040087117 Leitz et al. May 2004 A1
20040097022 Werkhoven et al. May 2004 A1
20040137167 Nguyen Jul 2004 A1
20040151845 Nguyen et al. Aug 2004 A1
20040157409 Ghyselen et al. Aug 2004 A1
20040178406 Chu Sep 2004 A1
20040192002 Soman et al. Sep 2004 A1
20040197945 Woelk et al. Oct 2004 A1
20040217845 Silver et al. Nov 2004 A1
20040219735 Brabant et al. Nov 2004 A1
20050051795 Arena et al. Mar 2005 A1
20050054175 Bauer Mar 2005 A1
20050067377 Lei et al. Mar 2005 A1
20050079692 Samoilov et al. Apr 2005 A1
20050081787 Im Apr 2005 A1
20050150447 Ghyselen et al. Jul 2005 A1
20050170577 Yao et al. Aug 2005 A1
20050191826 Bauer et al. Sep 2005 A1
20050192193 Korzenski et al. Sep 2005 A1
20050266700 Jursich et al. Dec 2005 A1
20050277260 Cohen et al. Dec 2005 A1
20060057825 Bude et al. Mar 2006 A1
20060138393 Seo et al. Jun 2006 A1
20060145188 Dantz et al. Jul 2006 A1
20060199357 Wan et al. Sep 2006 A1
20060211230 Figuet Sep 2006 A1
20060216417 Todd et al. Sep 2006 A1
20070044706 Kang et al. Mar 2007 A1
20070048956 Dip et al. Mar 2007 A1
20070051975 Figuet et al. Mar 2007 A1
20070117335 Sandhu et al. May 2007 A1
20070117398 Okada et al. May 2007 A1
20070134886 Quevedo-Lopez et al. Jun 2007 A1
20070155138 Tomasini et al. Jul 2007 A1
20070264801 Cody et al. Nov 2007 A1
20080017952 Cody et al. Jan 2008 A1
20090072271 Gomez et al. Mar 2009 A1
20090203197 Hanawa et al. Aug 2009 A1
20090305458 Hunks et al. Dec 2009 A1
20100006024 Brabant et al. Jan 2010 A1
20110117732 Bauer et al. May 2011 A1
20110256726 Lavoie et al. Oct 2011 A1
20110262660 Ishii et al. Oct 2011 A1
20110315992 Nguyen et al. Dec 2011 A1
20120009802 LaVoie et al. Jan 2012 A1
20120028410 Marsh Feb 2012 A1
20120028454 Swaminathan et al. Feb 2012 A1
20120231611 Gatineau et al. Sep 2012 A1
20120244688 Bauer et al. Sep 2012 A1
20120247386 Sanchez et al. Oct 2012 A1
20130045374 Yu et al. Feb 2013 A1
20130210217 Xiao Aug 2013 A1
20130233240 Cody et al. Sep 2013 A1
20140065841 Matero Mar 2014 A1
20140120738 Jung et al. May 2014 A1
Foreign Referenced Citations (20)
Number Date Country
0858101 Aug 1998 EP
1 681 711 Jul 2006 EP
04-245419 Sep 1992 JP
H07-037823 Feb 1995 JP
10-256169 Sep 1998 JP
2000-021783 Jan 2000 JP
2000-286413 Oct 2000 JP
2002-525255 Aug 2002 JP
2002-539613 Nov 2002 JP
2003-023146 Jan 2003 JP
2004-179452 Jun 2004 JP
2005-518093 May 2005 JP
2005-536876 Dec 2005 JP
2006-191112 Jul 2006 JP
WO 0015885 Mar 2000 WO
WO 200054338 Sep 2000 WO
WO 0141544 Jun 2001 WO
WO 02097864 Dec 2002 WO
WO 03069658 Aug 2003 WO
WO 2011027321 Mar 2011 WO
Non-Patent Literature Citations (93)
Entry
“Physics of Thin Films”, printed from http://www.uccs.edu/˜tchriste/courses/PHYS549/549lectures/film2.html (Feb. 22, 2000).
Bauer et al., “Crystalline to Amorphous Phase Transition in Very Low Temperature Molecular Beam Epitaxy”, Materials Science and Engineering B89:263-268 (2002).
Bauer et al., “High Ge content photodetectors on thin SiGe buffers”, Materials Science and Engineering B89:77-83 (2002).
Bauer et al., “Relaxed SiGe buffers with thicknesses below 0.1 μm”, Thin Solid Films 369:152-156 (2000).
Bensahel et al., “Single-wafer processing of in-situ doped polycrystalline Si and Si1-xGex”, Solid State Technology, pp. S5-S10 (Mar. 1998).
Bolkhovityanov et al., “Artificial GeSi Substrates for Heteroepitaxy: Achievements and Problems,” Semiconductors 37(5): 493-518 (2003).
Cannon, D. et al., “Tensile strained epitaxial Ge films on Si(100) substrates with potential application in L-band telecommunications,” Applied Physics Letters, vol. 84, No. 6, Feb. 9, 2004, pp. 906-908.
Christiansen et al., “Strain Relaxation Mechanisms in He+-Implanted and Annealed Si1-xGex Layers on Si(001) Substrates”, Material Research Society Symposium Proceedings 686:A1.6.1-A1.6.6 (2002).
Chui et al., “Ultrathin high-k gate dielectric technology for germanium MOS applications”, IEEE 60th Annual Device Research Conference (DRC) Digest, paper VII.B2, pp. 191-192 (2002).
Colace et al., “Ge/Si(001) photodetector for near infrared light”, Solid State Phenomena 54:55-58 (1997).
Colace et al., “Metal-Ge—Si diodes for near-infrared light detection”, Journal of Vacuum Science and Technology B 17:465 (1999).
Colace et al., “Metal-semiconductor-metal near-infrared light detector based on epitaxial Ge/Si”, Applied Physics Letters 72:3175-3177 (1998).
Colace, L. et al., “Efficient high-speed near-infrared Ge photodetectors integrated on Si substrates,” Applied Physics Letters, vol. 76, No. 10, Mar. 6, 2000, pp. 1231-1233.
Colace, L. et al., “Ge-on-Si Approaches to the Detection of Near-Infrared Light,” IEEE Journal of Quantum Electronics, vol. 35, No. 12, Dec. 1999, pp. 1843-1852.
Currie et al., “Controlling threading dislocation densities in Ge on Si using graded SiGe layers and chemical-mechanical polishing”, Applied Physics Letters 72:1718-1720 (1998).
Delhougne et al., “Development of a New Type of SiGe Thin Strain Relaxed Buffer Based on the Incorporation of a Carbon-Containing Layer”, Applied Surface Science 224:91-94 (2004).
Fama, S. et al., “High performance germanium-on-silicon detectors for optical communications,” Applied Physics Letters, vol. 81, No. 4, Jul. 22, 2002, pp. 586-588.
File History printed May 23, 2012 for U.S. Appl. No. 10/800,390, filed Mar. 12, 2004, entitled “Epitaxial Semiconductor Deposition Methods and Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 10/993,024, filed Nov. 18, 2004, entitled “Epitaxial Semiconductor Deposition Methods and Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 11/506,320, filed Aug. 18, 2006, entitled “Epitaxial Semiconductor Deposition Methods and Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 11/755,528, filed May 30, 2007, entitled “Epitaxial Semiconductor Deposition Methods and Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 12/556,377, filed Sep. 9, 2009, entitled “Epitaxial Semiconductor Deposition Methods and Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 11/067,307, filed Feb. 25, 2005, entitled “Germanium Deposition”.
File History printed May 23, 2012 for U.S. Appl. No. 11/867,318, filed Oct. 4, 2007, entitled “Germanium Deposition”.
File History printed May 23, 2012 for U.S. Appl. No. 11/388,313, filed Mar. 23, 2006, entitled “Heteroepitaxial Deposition Over an Oxidized Surface”.
File History printed May 23, 2012 for U.S. Appl. No. 11/431,336, filed May 9, 2006, entitled “Semiconductor Buffer Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 11/491,616, filed Jul. 24, 2006, entitled “Strained Layers Within Semiconductor Buffer Structures”.
File History printed May 23, 2012 for U.S. Appl. No. 12/562,029, filed Sep. 17, 2009, entitled “Strained Layers Within Semiconductor Buffer Structures”.
Fischetti et al., “Band structure, deformation potentials, and carrier mobility in strained Si, Ge, and SiGe alloys”, Journal of Applied Physics 80:2234-2252 (1996).
Fitzgerald et al., “Totally Relaxed Gex Si1-x Layers with Low Threading Dislocation Densities Grown on Si Substrates,” Appl. Phys. Lett. 59(7): 811-813 (1991).
Giovane et al., “Correlation between leakage current density and threading dislocation density in SiGe p-i-n diodes grown on relaxed graded buffer layers”, Applied Physics Letters 78:541-543 (2001).
Hackbarth et al., “Alternatives to Thick MBE-Grown Relaxed SiGe Buffers”, Thin Solid Films 369:148-151 (2000).
Hartmann et al., “Reduced pressure—chemical vapor deposition of Ge thick layers on Si(001) for 1.3-1.55-μm photodetection”, Journal of Applied Physics 95:5905-5913 (2004).
Haynes et al., “Composition Dependence of Solid-Phase Epitaxy in Silicon-Germanium Alloys: Experiment and Theory”, Physical Review B 51:7762-7771 (1995).
Herzog et al., “Si/SiGe n-MODFETs on Thin SiGe Virtual Substrates Prepared by Means of He Implantation”, IEEE Electron Device Letters, 23:485-487 (2002).
Huang et al., “Electron and Hole Mobility Enhancement in Strained SOI by Wafer Bonding”, IEEE Transactions on Electron Devices 49:1566-1571 (2002).
Huang et al., “SiGe-on-Insulator Prepared by Wafer Bonding and Layer Transfer for High-Performance Field-Effect Transistors”, Applied Physics Letters 78:1267-1269 (2001).
Hull, R., “Metastable strained layer configurations in the SiGe/Si system,” (1999) EMIS Datareviews, Series No. 24: Properties of SiGe and SiGe:C, edited by Erich Kasper et al., INSPEC (2000), Londonm, UK.
International Preliminary Report on Patentability for International Application No. PCT/US2007/072252, dated Nov. 3, 2008.
International Preliminary Report on Patentability for PCT/US2007/008879 dated Nov. 20, 2008.
International Search Report and Written Opinion for PCT Application No. PCT/US2007/072252 dated Dec. 19, 2007.
International Search Report and Written Opinion dated Feb. 6, 2015 in Application No. PCT/US2014/068387.
International Search Report for International Application No. PCT/US04/07564 dated Apr. 6, 2005.
International Search Report for PCT/US05/06150 dated Jun. 19, 2008.
Isella et al., “Low-energy plasma-enhanced chemical vapor deposition for strained Si and Ge heterostructures and devices” Solid State Electronics, Elsevier Science Publishers, Barking, GB, vol. 48, No. 8, Aug. 2004 (Aug. 2008), pp. 1317-1323.
Ishikawa et al., “Strain-induced band gap shrinkage in Ge grown on Si substrate,” Applied Physics Letters, vol. 82, No. 12, Mar. 31, 2003, pp. 2044-2046.
Jackson et al., “Gate-Self-Aligned p-Channel Germanium MISFET's”, IEEE Electron Device Letters 12:605-607 (1991).
Kamins et al., “Deposition of Three-Dimensional Germanium Islands on Si(001) by Chemical Vapor Deposition at Atmospheric and Reduced Pressures”, J. Appl. Phys. 81:211-219 (1997).
Kasper et al., “New virtual substrate concept for vertical MOS transistors”, Thin Solid Films 336:319-322 (1998).
Kasper, “Prospects of SiGe Heterodevices”, Journal of Crystal Growth 150:921-925 (1995).
Kutsukake et al., “Fabrication of SiGe-On-Insulator through Thermal Diffusion on Germanium on Si-on-Insulator Substrate”, Jpn. J. Appl. Phys. 42:L232-L234 (2003).
Langdo et al., “High quality Ge on Si by epitaxial necking”, Applied Physics Letter, vol. 76, No. 25, pp. 3700-3702, Jun. 19, 2000.
Lee et al., “Electron mobility characteristics of n-channel metal-oxide-semiconductor field-effect transistors fabricated on Ge-rich single- and dual-channel SiGe heterostructures”, Journal of Applied Physics 95:1550-1555 (2004).
Lee et al., “Growth of strained Si and strained Ge heterostructures on relaxed Si1-xGex by ultrahigh vacuum chemical vapor deposition,” J. Vac. Sci. Technol. B 22(1) (Jan./Feb. 2004).
Lee et al., “Strained Ge channel p-type metal-oxide-semiconductor field-effect transistors grown on Si1-xGex/Si virtual substrates”, Applied Physics Letters 79:3344-3346 (2001).
Lee et al., “Strained Si/strained Ge dual-channel heterostructures on Relaxed Si0.5Ge0.5 for symmetric mobility p-type and n-type metal-oxide-semiconductor field-effect transistors”, Applied Physics Letters 83:4202-4204 (2003).
Letertre et al., “Germanium-on-insulator (GeOI) structure realized by the Smart Cut™ technology”, MRS Proceedings, vol. 809 (2004).
Levinstein, Michael E., Rumyantsev, Sergey L, and Shur, Michael S., Properties of Advanced Semiconductor Materials GaN, AlN, InN, BN, SiC, SiGe, John Wiley & Sons, Inc., 149-187 (2011).
Li, Q, et al., “Selective growth of Ge on Si(100) through vias of SiO2 nanotemplate using solid source molecular beam epitaxy,” Applied Physics Letters, vol. 83, No. 24, Dec. 15, 2003, pp. 5032-5034.
Liszkay et al., “Strain Relaxation Induced by He-Implantation at the Si¬¬1-xGex/Si(100) Interface Investigated by Positron Annihilation”, Applied Surface Science 194:136-139 (2002).
Liu, J. et al., “Silicidation—induced band gap shrinkage in Ge epitaxial films on Si,” Applied Physics Letters, vol. 84, No. 5, Feb. 2, 2004, pp. 660-662.
Luan et al., “High-quality Ge epilayers on Si with low threading-dislocation densities”, Applied Physics Letters 75:2909-2911 (1999).
Luysberg et al., “Effect of Helium Ion Implantation and Annealing on the Relaxation Behavior of Pseudomorphic Si1-xGex Buffer Layers on Si(100) Substrates”, Journal of Applied Physics 92:4290-4295 (2002).
Lyutovich et al., “Interaction between point defects and dislocations in SiGe”, Solid State Phenomena 69-70:179-184 (1999).
Lyutovich et al., “Relaxed SiGe buffer layer growth with point defect injection”, Materials Science and Engineering B71:14-19 (2000).
Lyutovich et al., “Thin SiGe buffers with high Ge content for n-MOSFETs”, Materials Science and Engineering B89:341-345 (2002).
Masini, G. et al.; “High-Performance p-i-n Ge on Si Photodetectors for the Near Infrared: From Model to Demonstration,” IEEE Transactions of Electron Devices, vol. 48, No. 6, Jun. 2001, pp. 1092-1096.
Medeiros-Ribeiro et al., “Equilibrium Size Distributions of Clusters During Strained Epitaxial Growth”, Materials Science and Engineering B67:31-38 (1999).
Nakamura et al., “InGaN/GaN/A1GaN-Based Laser Diodes with Modulation-Doped Strained-Layer Superlattices”, Jap. J. Appl. Phys., vol. 36, No. 12A, Part 2, p. L1568-L1571 (1997).
Nam et al., “Lateral epitaxy of low defect density GaN layers via organometallic vapor phase epitaxy”, Phys. Lett, vol. 71, No. 18, p. 2638 (1997).
Ni et al., “X-ray reciprocal space mapping studies of strain relaxation in thin SiGe layers (≤100 nm) using a low temperature growth step”, Journal of Crystal Growth 227-228:756-760 (2001).
Obata et al., “Structural Characterization of Si0.7Ge0.3 Layers Grown on Si(001) Substrates by Molecular Beam Epitaxy,” J. Appl. Phys. 81(1): 199-204 (1997).
Osten et al., “Relaxed Si1-xGex-Si1-x-yGexCy Buffer Structures with Low Threading Dislocation Density”, Applied Physics Letters 70:2813-2815 (1997).
Pending U.S. Appl. No. 11/267,494 entitled: Semiconductor Heterostructure and Method for Forming a Semiconductor Heterostructure, filed Mar. 11, 2005 by Christophe Figuet and Mark Kennard.
Pending U.S. Appl. No. 11/146,572 entitled: Laminated Layer Structure and Method for Forming the Same, filed Jun. 6, 2005 by Christophe Figuet.
Perego et al, “Fabrication of GeO2 layers using a divalent Ge precursor,” Applied Physics Letters 90, 2007.
Presting et al., “Buffer Concepts of Ultrathin Simgen Superlattices” Thin Solid Films, Elsevier-Sequoia S.A. Lausanne, CH, vol. 222, No. ½, Dec. 20, 1992 (Dec. 20, 1992), pp. 215-220.
Profijt et al., “Plasma-assisted atomic layer deposition: basics, opportunities and challenges”, J. Vac. Sci. Technol. A, vol. 29, No. 5, pp. 050801-1 050801-26.
Reinking et al., “Ge p-MOSFETs compatible with Si CMOS-technology”, Proceedings of the 29th ESSDERC 99:300-303 (1999).
Samavedam et al., “High-quality germanium photodiodes integrated on silicon substrates using optimized relaxed graded buffers”, Applied Physics Letters 73:2125-2127 (1998).
Schöllhorn et al., “Coalescence of germanium islands on silicon”, Thin Solid Films 336:109-111 (1998).
Shang et al., “Electrical characterization of germanium p-channel MOSFETs”, IEEE Electron Device Letters 24:242-244 (2003).
Singapore Search Report dated Jun. 16, 2009, received in Singapore Application No. 200809179-5, filed Jun. 27, 2007. 572VSG.
Singapore Written Opinion dated Jun. 16, 2009, received in Singapore Application No. 200809179-5, filed Jun. 27, 2007. 572VSG.
Sugii et al., “SiGe-on-Insulator Substrate Fabricated by Melt Solidification for a Strained-Silicon Complementary Metal-Oxide-Semiconductor”, J. Vac. Sci. Technol. B20(5):1891-1896 (2002).
Sugiyama et al., “Formation of Strained-Silicon Layer on Thin Relaxed-SiGe/SiO2/Si Structure Using SIMOX Technology”, Thin Solid Films 369:199-202 (2000).
Taiwanese Office Action dated Apr. 30, 2010 for Taiwanese Patent Application No. 093106618.
Teichert et al., “Interplay of Dislocation Network and Island Arrangement in SiGe Films Grown on Si(001)”, Thin Solid Films 380:25-28 (2000).
Thomas et al., “Structural characterization of thick, high-quality epitaxial Ge on Si substrates grown by low-energy plasma-enhanced chemical vapor deposition”, Journal of Electronic Materials 32:976-980 (2003).
Trinkaus et al., “Strain Relaxation Mechanism for Hydrogen-Implanted Si1-xGex/Si(100)Heterostructures”, Applied Physics Letters 76:3552-3554 (2000).
Vescan et al., “Relaxation Mechanism of Low Temperature SiGe—Si(100) Buffer Layers”, ICSI3, p. 141 (Mar. 2003).
Wolf, “Silicon Processing for the VLSI Era”, vol. 1: Process Technology, pp. 198 & 519-520 (1986).
Yamamoto et al., “Dislocation Structures and Strain-Relaxation in SiGe Buffer Layers on Si (0 0 1) Substrates with an Ultra-Thin Ge Interlayer,” Appl. Surface Sci. 224: 108-112 (2004).
Related Publications (1)
Number Date Country
20200266053 A1 Aug 2020 US
Provisional Applications (2)
Number Date Country
61713082 Oct 2012 US
61697007 Sep 2012 US
Continuations (2)
Number Date Country
Parent 14867833 Sep 2015 US
Child 16773026 US
Parent 13802393 Mar 2013 US
Child 14867833 US