This invention relates to multi-layered structures and methods of forming multi-layered structures.
As information processing apparatuses are developed, integrated circuit devices have been improved to operate with reduced response speeds. One method that may improve the response speed of an integrated circuit device is to increase the integration of cells on a single chip.
The need for increased speed and reduction in size has led to extensive research of capacitors. Generally, capacitors of an integrated circuit device include a bottom electrode, a dielectric layer formed on the bottom electrode, and a top electrode formed on the dielectric layer. Deposition processes are usually performed to form capacitors.
The formation of capacitors as illustrated in
Therefore, it is desirable to develop methods for forming structures lacking an interface oxide film between an electrode and a dielectric layer. In addition, it is desirable to develop methods for forming such structures in a single deposition apparatus.
Embodiments of the present invention can include multi-layered structures formed in a single atomic-layer deposition chamber. The temperature of the deposition chamber may be predetermined such that all of the processes required to form the multi-layered structures may be carried out in the deposition chamber. The formation of metal oxide layers in the multi-layered structures may be performed with water vapor or an oxidizing agent having a low oxidation power to inhibit the formation of unwanted oxide layers.
According to some embodiments of the present invention, a method for forming a multi-layered structure using an atomic layer deposition process includes the formation of a first metal oxide film over a substrate followed by the formation of a second metal oxide film over the first metal oxide film. The first metal oxide film is formed from oxidation of a first metal absorption film using water vapor or an oxidizing agent having a low oxidation power with respect to the substrate. The formation of the metal oxide film using water vapor inhibits the formation of an interlayer oxide layer between the metal oxide film and a substrate on which the metal oxide film is formed. A second metal oxide film can be formed over the first metal oxide film by the ozone oxidation of a second metal absorption film.
According to other embodiments of the present invention, multi-layered structures include multiple layers formed from the metal oxide films. Methods for forming the multi-layered structures having multiple metal layers include the formation of multiple metal layers wherein each metal layer includes one or more first metal oxide films and one or more second metal oxide films. The first metal oxide films can be formed by oxidizing a first metal absorption layer with water vapor. The second metal oxide films can be formed by oxidizing second metal absorption films with ozone. The use of water vapor as an oxidizing agent can inhibit the formation of interlayer oxides. Each metal layer can be formed to a desired thickness by depositing multiple first metal oxide films and second metal oxide films.
According to other embodiments of the present invention, a capacitor can be formed having a multi-layered dielectric layer. The multi-layered dielectric layer can include one or more first metal oxide films and one or more second metal oxide films. The metal oxide films can be formed according to embodiments of the present invention using water vapor as an oxidizing agent and ozone as a second oxidizing agent. The multi-layered dielectric layers can be void of interlayer oxide films due to the use of water vapor as the oxidizing agent.
The invention can be more readily ascertained from the following description of the invention when read in conjunction with the accompanying drawings in which:
The present invention now will be described more fully hereinafter with reference to the accompanying drawings, in which embodiments of the invention are shown. This invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art. In the drawings, the thickness of layers and regions are exaggerated for clarity. Like numbers refer to like elements throughout. It will be understood that when an element such as a layer, region or substrate is referred to as being “on” or “onto” another element, it can be directly on the other element or intervening elements may also be present. When an element such as a layer, region or substrate is referred to as being “directly on” another element, it is in direct contact with that other element.
Embodiments of the present invention include methods for forming multi-layered structures and multi-layered structures formed by these methods. In some embodiments, the multi-layered structures are formed using atomic layer deposition processes. In other embodiments, the multi-layered structures are formed in a closed system or a single chamber. The thickness of the layers of the multi-layered structures formed according to embodiments of the present invention can be adjusted as desired for a particular application by varying deposition conditions in the atomic layer deposition process.
Embodiments of the present invention can also include methods for forming a multi-layered structure includes the deposition of multiple layers using an atomic layer deposition process. Two or more layers of metal oxides can be formed on a substrate using an atomic layer deposition process wherein a first metal layer is deposited on the substrate and oxidized to form a first metal oxide layer, followed by the deposition of a second metal layer on the first metal oxide layer and oxidation of the second metal layer to form a second metal oxide layer. Additional metal oxide layers can be formed on the second metal oxide layer using the same processes as used to deposit the first and second metal oxide layers.
The formation of multiple metal oxide layers on a substrate can be performed in an atomic layer deposition chamber. In some embodiments, the formation of the multiple metal oxide layers can be performed in a single atomic layer deposition chamber to improve the efficiency of the process. In addition, the temperature and pressure of the atomic layer deposition chamber can be adjusted to allow different metal oxide layers to be deposited on a substrate at different or varying temperatures and pressures as desired.
According to some embodiments of the present invention, a method for forming a multi-layered structure using an atomic layer deposition process can include the formation of a first metal oxide film over a substrate followed by the formation of a second metal oxide film over the first metal oxide film. The first metal oxide film can be deposited on a substrate in an atomic layer deposition chamber by the formation of a first absorption film on the substrate followed by the oxidization of the first absorption film to form the first metal oxide film. The second metal oxide film can be deposited on the first metal oxide film by the formation of a second absorption film over the first metal oxide film followed by the oxidation of the second absorption film.
The first absorption film can be deposited on a substrate loaded into an atomic layer deposition chamber by the introduction of a first metal precursor into the deposition chamber using an inert gas as a carrier gas. Portions of the first metal precursor introduced into the deposition chamber settle on a surface of the substrate. Those portions of the first metal precursor that do not form the first absorption film on the substrate are purged from the deposition chamber so that the first absorption film is formed on the substrate. An inert gas may be used as a purge gas.
In some embodiments, a first oxidizing agent can be introduced into the deposition chamber to oxidize the first absorption film on the substrate surface. The introduction of the oxidizing agent can occur after an unused portion of the first metal precursor is removed from the deposition chamber. The first oxidizing agent reacts with the first metal precursor to form a first metal oxide film. Any first oxidizing agent that does not react with the first absorption film to produce the first metal oxide film is purged from the deposition chamber.
A second absorption film can be deposited on the first metal oxide film by the introduction of a second metal precursor into the deposition chamber following a purge of the first oxidizing agent. Portions of the second metal precursor introduced into the deposition chamber are formed on a surface of the first metal oxide film, forming a second absorption film on the first metal oxide film. The second absorption film is formed on the first metal oxide film by chemisorption, physisorption, or a combination of chemisorption and physisorption. Those portions of the second metal precursor that do not form the second absorption film on the first metal oxide film are purged from the deposition chamber.
A second oxidizing agent can be introduced into the deposition chamber to oxidize the second absorption film. The introduction of the second oxidizing agent can occur after an unused portion of the second metal precursor is removed from the deposition chamber. The second oxidizing agent reacts with the second metal precursor to form a second metal oxide film on the first metal oxide film. Those portions of the second oxidizing agent that do not react with the second absorption film to produce the second metal oxide film are purged from the deposition chamber.
The temperature of the deposition chamber can be set at a pre-determined temperature prior to the introduction of the first metal precursor into the deposition chamber. According to embodiments of the present invention, the temperature within the deposition chamber can be between about 100° C. to about 700° C. In other embodiments, the temperature of the deposition chamber can be maintained at between about 250° C. and about 450° C. during the deposition and oxidation of the first and second metal oxide layers. The use of a predetermined temperature in the deposition chamber for each step in the processes of the present invention allows the formation of multi-layered structures using a single chamber even though several kinds of reactants can be used in the formation of the multi-layered structure.
The first and second metal precursors include metal precursors that can be used in the formation of semi-conductor and microelectronic devices. For example, the metal precursors can include, but are not limited to, tantalum (Ta) compounds, hafnium (Hf) compounds, titanium (Ti) compounds, aluminum (Al) compounds, and lanthanum (La) compounds. A combination of metal precursors can be selected to form the layers of a multi-layered structure based upon the desired characteristics of the structure. For example, aluminum oxide films may generate low leakage currents and have relatively low dielectric constants. Hafnium oxide films and titanium oxide films may exhibit a relatively high dielectric constant as well as a relatively high leakage current. By creating different layers of films the characteristics of the multi-layered structure can be altered. Therefore, multi-layered structures having hafnium-aluminum oxide films or titanium-aluminum oxide films may exhibit low leakage current and high dielectric constants.
The first oxidizing agents used with embodiments of the present invention can include oxidizing agents having a low oxidation power relative to the substrate such as water vapor and the second oxidizing agents used with embodiments of the present invention can include oxidizing agents having a high oxidation power relative to the first oxidizing agents such as ozone. The use of water vapor as an oxidizing agent to oxidize a metal absorption film on a substrate helps to prevent the formation of an oxide layer between the formed metal oxide layer and the substrate.
A cross-sectional view of a multi-layered structure formed according to embodiments of the present invention is illustrated in
As illustrated in
As illustrated in
A second metal oxide film 250 is formed over the first metal oxide film 245 as illustrated in
Multiple thin layers may be formed on a substrate by repeating the process steps described with respect to
As illustrated in
Reactive components that are removed from the deposition chamber according to processes of the present invention may be removed by known methods, for instance, by purging the deposition chamber with an inert gas. Reactive components that may be removed this way include, for example, metal precursors and oxidizing agents.
In other embodiments of the present invention multi-layered structures include multiple layers of the metal oxide films. Methods for forming the multi-layered structures having multiple metal layers include the formation of multiple metal layers wherein each metal layer includes one or more first metal oxide films and one or more second metal oxide films. Each metal layer is formed to a desired thickness by depositing multiple first metal oxide films and second metal oxide films.
An example of the formation of a multi-layered structure having metal layers according to some embodiments of the present invention is illustrated in
Referring to
The first metal oxide film 245 can include, for example, an aluminum oxide film formed by the oxidation of a trimethylaluminum absorption layer using water vapor. A trimethylaluminum absorption film is deposited using trimethylaluminum as the first metal precursor. The use of water vapor as a first oxidizing agent oxidizes the trimethylaluminum and prevents the formation of an oxide layer between the first metal oxide film 245 and the substrate 200.
A second metal oxide film 250 is then formed over the first metal oxide film 245 as illustrated in
For example, a hafnium chloride metal precursor may be introduced into the deposition chamber to form a hafnium chloride second absorption layer over the first metal oxide film. Ozone introduced as the second oxidizing agent rapidly oxidizes the hafnium chloride absorption layer, forming the second metal oxide film 250.
According to some embodiments of the present invention, the combination of the first metal oxide film and the second metal oxide film form a first metal layer 260 as illustrated in
In other embodiments of the present invention, a second metal layer 290 is formed on the first metal layer 260 as illustrated in
For example, trimethylaluminum can be used as the third metal precursor to form a trimethylaluminum absorption layer on the first metal layer 260. Water vapor introduced as an oxidizing agent oxidizes the trimethylaluminum, forming an aluminum oxide third metal oxide film 275. The third metal oxide film 275 is formed with the formation of an oxide layer between the third metal oxide film 275 and the first metal layer 260.
A fourth metal oxide film 280 is then formed over the third metal oxide film 275 as illustrated in
For example, a hafnium chloride metal precursor may be introduced into the deposition chamber to form a hafnium chloride fourth absorption layer over the third metal oxide film 275. Ozone introduced as the oxidizing agent rapidly oxidizes the hafnium chloride absorption layer, forming the fourth metal oxide film 280.
According to embodiments of the present invention, the combination of the third metal oxide film 275 and the fourth metal oxide film 280 form a second metal layer 290 as illustrated in
Additional metal layers may be formed on the second metal layer 290 as desired by consecutively repeating the processes illustrated in
The use of water vapor as an oxidizing agent to form the first metal oxide films and third metal oxide films according to embodiments of the present invention suppresses the formation of oxide films between the first metal oxide films and the substrate and the third metal oxide films and the first metal layer. Thus, according to some embodiments of the present invention, there are no oxide films separating a substrate 200 from a first metal layer 260 or separating the metal layers such as a first metal layer 260 and a second metal layer 290.
According to other embodiments of the present invention, a capacitor can be formed. An example of the formation of a capacitor according to embodiments of the present invention is illustrated in
A second insulation film 340 is deposited over the first insulation film 310 and the contact plugs 330 as illustrated in
As illustrated in
Portions of the third insulation film 355 and the conductive film 350 are removed from the structure by a chemical mechanical polishing process, or other known process, until the second insulation film 340 is exposed as illustrated in
The second insulation film 340 and the inner insulation film patterns 355a are removed from the structure to expose the bottom electrodes 350a formed over the contact plugs 330 as illustrated in
A buffer layer (not shown) may be formed on the bottom electrodes 350a to prevent reaction or diffusion between the bottom electrodes 350a and a dielectric film subsequently formed on the bottom electrodes 350a. For example, a buffer layer can be formed on a bottom electrode 350a formed of polysilicon, silicon oxide, silicon nitride, or silicon oxynitride by a rapid thermal nitration (RTN) process or a rapid thermal oxidation (RTO) process. A buffer layer formed by an RTN process is performed at a temperature between about 500° C. to about 900° C. in a nitrogen (N2) or an ammonia (NH3) atmosphere. A buffer layer formed by an RTO process is performed at a temperature between about 500° C. and about 900° C. in an oxygen (O2) or a dinitrogen monoxide (N2O) atmosphere. The activation energy for forming the buffer layer can be lowered by providing a light energy such as a plasma or an ultra violet light on the reactant.
The formation of a buffer layer can reduce the deterioration of a dielectric film on the bottom electrodes 350a. In addition, a buffer layer can decrease leakage current by dissipating an electric field directly applied to a dielectric film formed on the bottom electrodes 350a.
According to embodiments of the present invention, a dielectric film is formed on the structure illustrated in
According to other embodiments of the present invention, the dielectric layer 360 includes multiple metal layers formed according to embodiments of the present invention. For instance, in some embodiments a dielectric layer 360 having multiple metal layers is formed by methods similar to those described with respect to
The dielectric layers 360 formed according to embodiments of the present invention are formed in an atomic-layer deposition chamber set at a predetermined temperature between about 100° C. and about 700° C. In some embodiments, the temperature in the deposition chamber may be between about 250° C. and 450° C.
The first absorption films are oxidized to form the first metal oxide film using water vapor as the first oxidizing agent. The use of water vapor as the first oxidizing agent inhibits the formation of an oxide layer between the first metal oxide film and the substrate on which it is deposited, for example the bottom electrode 350a or a buffer layer thereon. The second absorption films are oxidized using ozone as an oxidizing agent. The use of ozone as an oxidizing agent results in a faster oxidation of the second absorption films than the first absorption films. Inert purge gases are used to remove the first and second metal precursors and the oxidizing agents from the deposition chamber.
The dielectric layers 360 formed according to embodiments of the present invention are multi-layered structures that can include different metal oxides, such as, but not limited to, tantalum oxides, hafnium oxides, titanium oxides, aluminum oxides, or lanthanum oxides. In some embodiments of the present invention the dielectric layers 360 have a high dielectric constant.
After a dielectric layer 360 is formed according to embodiments of the present invention, it can be thermally treated under an oxygen atmosphere. A plasma or an ultra violet ray can be applied during the thermal treatment as an additional source of energy. In addition, argon (Ar), nitrogen (N2), hydrogen (H2), helium (He), oxygen (02), ozone (03), or ammonia (NH3) may be provided to the dielectric layer 360. The thermal treatment improves the density of the dielectric layer 360 and effectively prevents the generation of leakage current from the dielectric layer 360.
illustrated in
Multi-layered structures formed according to embodiments of the present improved characteristics which result from the methods of forming the multi-layered structures. For instance, the multi-layered structures exhibit excellent electrical characteristics and lack oxide layers at the interfaces between a substrate and the metal oxide layers. In addition, oxide layers do not form between the metal oxide layers due to the methods by which the multi-layered structures are formed. Furthermore, the ability to form the multi-layered structures in a single deposition chamber at a predetermined temperature according to embodiments of the present invention improves the efficiency of the production process and reduces cost associate with the production of multi-layered structures.
Having thus described certain embodiments of the present invention, it is to be understood that the invention defined by the appended claims is not to be limited by particular detail set forth in the above description as many apparent variations thereof are possible without departing from the spirit or scope thereof as hereinafter claimed.