The present disclosure generally relates to processes for manufacturing electronic devices. More particularly, the disclosure relates to forming a Transition Metal Silicate film through atomic layer deposition (ALD).
Atomic layer deposition (ALD) is a method for depositing a thin film on a substrate through sequential distribution of various precursors. A conventional ALD method can take place in a reaction system comprising a reaction chamber, a substrate holder, a gas flow system, and an exhaust system. Growth of the thin film takes place when the precursors adsorb onto active sites on the substrate such that only a monolayer of the precursor forms on the substrate. Any excess precursor may then be expunged from the reaction chamber through the exhaust. Another precursor may be introduced to form another monolayer. The process may be repeated as needed to form a desired film of a desired thickness.
ALD processes have been particularly effective in forming gate dielectrics in complementary metal oxide semiconductor (CMOS) devices. For many years, silicon oxide (SiO2) has been used for components in CMOS applications as transistor gate dielectrics and gate dielectrics. However, with the reduction in size of the components, SiO2 has demonstrated problematic effects in the form of increased leakage currents. Controlling leakage current with the size constraints has proved challenging for SiO2.
In the formation of gate dielectrics, a dielectric material with a high dielectric constant (“high-k dielectric”) has been shown to have the performance characteristics in order to achieve smaller device geometries while controlling leakage and other electrical criteria. With these desired goals in mind, U.S. Pat. No. 7,795,160 to Wang et al. discloses methods for controlled deposition of a conformal metal silicate film onto a substrate surface. Going away from the prior SiO2 methods, the methods disclosed could be used to form, specifically, hafnium silicate (HfSiOx) and zirconium silicate (ZrSiOx) films for various applications, such as gate stacks in CMOS devices, dielectric layers in DRAM devices and components of other capacitor-based devices. HfSiOx and ZrSiOx offer thermal stability and device performance in integrated circuits in smaller device geometries.
Also going away from prior SiO2 methods, U.S. Pat. No. 8,071,452 to Raisanen discloses a method for ALD deposition of a metal film layer in order for use in high-k dielectric materials. Specifically, a method for depositing a hafnium lanthanum oxide (HfLaO) layer is disclosed. The method allows a HfLaO dielectric layer to be engineered with a desired dielectric constant and/or other controllable characteristics.
As a result, a method for forming a transition metal film that attains desired dielectric constants as well as demonstrates reliability is desired.
In accordance with at least one embodiment of the invention, a method of forming a film is disclosed. The method comprises: providing a substrate for processing in a reaction chamber; performing a silicon precursor deposition onto the substrate; and performing a metal precursor deposition onto the substrate; wherein the silicon precursor deposition step is performed X times; wherein the metal precursor deposition step is performed Y times; wherein a transition metal silicate film is formed; wherein a metal precursor from the metal precursor deposition step comprises a metal atom bonded to a nitrogen atom or a carbon atom.
In accordance with at least one embodiment of the invention, a method of forming a transition metal silicate film is disclosed. The method comprises: providing a substrate for processing in a reaction chamber; performing a silicon precursor deposition onto the substrate, the performing the silicon precursor deposition comprising: pulsing a silicon precursor; purging the silicon precursor from the reaction chamber with a purge gas; pulsing an oxidizing precursor; and purging the oxidizing precursor from the reaction chamber with the purge gas; performing a metal precursor deposition onto the substrate, the performing the metal precursor deposition comprising: pulsing a metal precursor; purging the metal precursor from the reaction chamber with a purge gas; pulsing an oxidizing precursor; and purging the oxidizing precursor from the reaction chamber with the purge gas; wherein the silicon precursor deposition step is repeated X times; wherein the metal precursor deposition step is repeated Y times; and wherein a transition metal silicate film is formed; wherein the metal precursor comprises a metal atom bonded to a nitrogen atom or a carbon atom.
For purposes of summarizing the invention and the advantages achieved over the prior art, certain objects and advantages of the invention have been described herein above. Of course, it is to be understood that not necessarily all such objects or advantages may be achieved in accordance with any particular embodiment of the invention. Thus, for example, those skilled in the art will recognize that the invention may be embodied or carried out in a manner that achieves or optimizes one advantage or group of advantages as taught or suggested herein without necessarily achieving other objects or advantages as may be taught or suggested herein.
All of these embodiments are intended to be within the scope of the invention herein disclosed. These and other embodiments will become readily apparent to those skilled in the art from the following detailed description of certain embodiments having reference to the attached figures, the invention not being limited to any particular embodiment(s) disclosed.
These and other features, aspects, and advantages of the invention disclosed herein are described below with reference to the drawings of certain embodiments, which are intended to illustrate and not to limit the invention.
It will be appreciated that elements in the figures are illustrated for simplicity and clarity and have not necessarily been drawn to scale. For example, the dimensions of some of the elements in the figures may be exaggerated relative to other elements to help improve understanding of illustrated embodiments of the present disclosure.
Although certain embodiments and examples are disclosed below, it will be understood by those in the art that the invention extends beyond the specifically disclosed embodiments and/or uses of the invention and obvious modifications and equivalents thereof. Thus, it is intended that the scope of the invention disclosed should not be limited by the particular disclosed embodiments described below.
In at least one embodiment of the invention, the order of the subcycles may be varied such that an order of the subcycles could be in a sandwich structure. For example, if pulse ratio of the silicon oxide subcycle to the lanthanum oxide subcycle equals 2:1; then precursor deposition may proceed as one silicon oxide subcycle 100, followed by a lanthanum oxide subcycle 200, and then a silicon oxide subcycle 100. In another embodiment of the invention, the order of the subcycles could be such that either subcycle could be first or last. Subcycles may be inserted at non-fixed ratios in order to effectively grade a composition of the film versus a vertical distance from the substrate.
It may also be possible that different orders for subcycles result in a film with the similar properties.
In other embodiments consistent with the invention, the oxygen precursor pulse/purge 120 may involve a pulse and purge of at least one of: water (H2O); diatomic oxygen (O2); hydrogen peroxide (H2O2); ozone (O3); oxygen plasma; atomic oxygen (O); oxygen radicals; or methyl alcohol (CH3OH). It may be possible that different oxidizing precursors could be used for the different cycles; for example, O3 may be used for the silicon oxide subcycle, while water can be used for the lanthanum oxide subcycle. In other embodiments of the invention, it may be possible to use an oxygen source that does not comprise ozone, O2, H2O2, H2O, methyl alcohol, or oxygen plasma.
In at least one embodiment of the invention, a metal precursor in the metal precursor pulse/purge 210 may be one of the following: an amidinate based precursor, such as Lanthanum formamidinate (La(FAMD)3) or tris(N,N′-diisopropylacetamidinato)lanthanum (La(iPrAMD)3); a diketonate precursor, such as (La(THD)3); a Cp(cyclopentadienyl)-based precursor such as Tris(isopropyl-cyclopentadienyl)lanthanum (La(iPrCp)3); or an amido-based chemistry such as tris(bistrimethylsilylamido)-lanthanum (La[N(SiMe3)2]3); or hybrid combinations of the above. In other embodiments consistent with the invention, the metal precursor may be a lanthanum or other rare earth metal precursor having a bond between nitrogen, such as a lanthanum amidinate, for example. The amidinate compounds may comprise delocalized electrons that result in the bond between the nitrogen and the lanthanum or rare earth metal. In other embodiments consistent with the invention, the metal precursor may be a lanthanum or other rare earth metal precursor having a bond with carbon, such as a lanthanum cyclopentadienyl, for example. This metal precursor may comprise delocalized electrons, which are considered to be compounds, in which the bond between the carbon and the lanthanum or rare earth forms. In other embodiments consistent with the invention, the metal precursor may be a lanthanum or other rare earth metal precursor having a bond with both nitrogen and carbon, such as a lanthanum amidinate and a lanthanum cyclopentadienyl compound, for example.
In other embodiments consistent with the invention, the oxygen precursor pulse/purge 220 may involve at least one of: water (H2O), diatomic oxygen (O2), hydrogen peroxide (H2O2), ozone (O3), oxygen plasma, oxygen radicals, atomic oxygen, or methyl alcohol (CH3OH). The metal oxide subcycle 200 may be substituted with an yttrium oxide subcycle or another element's subcycle depending on what is the final desired product. Other elements could be lanthanides, erbium, erbium oxide, magnesium, magnesium oxide, scandium, or scandium oxide, among others. These other materials may also be preferable as they demonstrate an ability to cause the Vt shift. For yttrium, the yttrium subcycle may comprise a yttrium pulse, a purge of the yttrium precursor, a H2O pulse, and a purge of the H2O precursor. The yttrium precursor could be one of the following: a Cp(cyclopentadienyl)-based chemistry, such as Y(EtCp)3 and tris(methylcyclopentadienyl)yttrium (Y(MeCp)3); an amidinate-based precursor, such as Tris(N,N′-diisopropylacetamidinato) Yttrium (TDIPAY); a diketonate precursor, such as (Y(THD)3) and tris(2,2,6,6-tetramethyl-3,5-octanedionato)Yttrium (Y(tmod)3); or an amide-based precursor, such as Tris[N,N-bis(trimethylsilyl)amide]yttrium. Typical temperatures for this process range from 100-450° C., or from 150-400° C., or from 175-350° C., or from 200-300° C., with pressures ranging from 1 to 10 Torr.
The pulse ratio X:Y of the silicon and metal oxide subcycles can allow for incorporation of Silicon (Si) into the metal silicate film. The pulse ratio X:Y may range to be 5:1, 7:1, 10:1, and 20:1.
An additional benefit attained through at least one embodiment of the invention includes a lower carbon impurity level. Carbon is considered as a trap center and may degrade the performance of a device formed using the deposited film. As a result, a lower carbon level may be preferable.
Carbon may be formed easily if strong oxygen reactants, such as ozone or oxygen plasmas, are used. These strong reactants may result in greater oxidation of the substrate. Conventional LaOx films deposited through ALD indicate a high carbon impurity level between 15-20%. In addition, conventional LaOx films may also show high hydroxide impurities as well as low silicon incorporation.
In accordance with at least one embodiment of the invention, a combination of a silicon halide precursor, a rare earth precursor having a bond with a nitrogen/carbon atom, a proper oxygen precursor (such as water), and a high mobility channel material may be the reason for a lower carbon impurity level. The proper oxygen precursor may result in less oxidation of the substrate, potentially providing for a good surface or interface for subsequent deposition of additional materials, such as a high-k material formed by ALD.
As shown in
In accordance with at least one embodiment of the invention, a lanthanum hydroxide film (La(OH)3) may be formed. In at least one embodiment of the invention, for a pure lanthanum hydroxide (La(OH)3) film, the hydrogen content could be less than 43%. In accordance with at least one embodiment of the invention, a lanthanum hydroxide film may have hydrogen impurities, ranging from less than 20 mol-% of hydroxide (OH), less than 15 mol-% of hydroxide (OH), less than 10 mol-% of hydroxide (OH), or less than 5 mol-% of hydroxide (OH).
The particular implementations shown and described are illustrative of the invention and its best mode and are not intended to otherwise limit the scope of the aspects and implementations in any way. Indeed, for the sake of brevity, conventional manufacturing, connection, preparation, and other functional aspects of the system may not be described in detail. Furthermore, the connecting lines shown in the various figures are intended to represent exemplary functional relationships and/or physical couplings between the various elements. Many alternative or additional functional relationship or physical connections may be present in the practical system, and/or may be absent in some embodiments.
It is to be understood that the configurations and/or approaches described herein are exemplary in nature, and that these specific embodiments or examples are not to be considered in a limiting sense, because numerous variations are possible. The specific routines or methods described herein may represent one or more of any number of processing strategies. Thus, the various acts illustrated may be performed in the sequence illustrated, in other sequences, or omitted in some cases.
The subject matter of the present disclosure includes all novel and nonobvious combinations and subcombinations of the various processes, systems, and configurations, and other features, functions, acts, and/or properties disclosed herein, as well as any and all equivalents thereof.
The present application claims priority to U.S. Provisional Patent Application No. 62/242,804, entitled “Implementing Atomic Layer Deposition Gate Dielectrics for MOSFET Devices” and filed on Oct. 16, 2015, the contents of which are hereby incorporated herein by reference, to the extent such contents do not conflict with the present disclosure.
| Number | Date | Country | |
|---|---|---|---|
| 62242804 | Oct 2015 | US |