1. Field of the Invention
Embodiments of the invention relate to the processing of semiconductor substrates. More particularly, embodiments of the invention relate to deposition of tungsten layers on semiconductor substrates using vapor deposition techniques.
2. Description of the Related Art
The semiconductor processing industry continues to strive for larger production yields while increasing the uniformity of layers deposited on substrates having larger surface areas. These same factors in combination with new materials also provide higher integration of circuits per unit area of the substrate. As circuit integration increases, the need for greater uniformity and process control regarding layer thickness rises. As a result, various technologies have been developed to deposit layers on substrates in a cost-effective manner, while maintaining control over the characteristics of the layer.
Chemical vapor deposition (CVD) is one of the most common deposition processes employed for depositing layers on a substrate. CVD is a flux-dependent deposition technique that requires precise control of the substrate temperature and the precursors introduced into the processing chamber in order to produce a desired layer of uniform thickness. These requirements become more critical as substrate size increases, creating a need for more complexity in chamber design and gas flow technique to maintain adequate uniformity.
A variant of CVD that demonstrates excellent step coverage is cyclical deposition or atomic layer deposition (ALD). Cyclical deposition is based upon atomic layer epitaxy (ALE) and employs chemisorption techniques to deliver precursor molecules on a substrate surface in sequential cycles. The cycle exposes the substrate surface to a first precursor, a purge gas, a second precursor and the purge gas. The first and second precursors react to form a product compound as a film on the substrate surface. The cycle is repeated to form the layer to a desired thickness.
Formation of film layers at a high deposition rate while providing adequate step coverage are conflicting characteristics often necessitating the sacrifice of one to obtain the other. This conflict is true particularly when refractory metal layers are deposited over gaps or vias during the formation of contacts interconnecting adjacent metallic layers separated by dielectric layers. Historically, CVD techniques have been employed to deposit conductive material such as refractory metals in order to inexpensively and quickly form contacts. Due to the increasing integration of semiconductor circuitry, tungsten has been used based upon superior step coverage. As a result, deposition of tungsten employing CVD techniques enjoys wide application in semiconductor processing due to the high throughput of the process.
Depositing tungsten by conventional CVD methods, however, is attendant with several disadvantages. For example, ALD processes deposit tungsten films into vias containing high aspect ratios (e.g., 20), whereas conventional CVD processes will usually cause similar vias to “pinch-off” and not completely fill. Also, blanket deposition of a tungsten layer on a semiconductor wafer is time-consuming at temperatures below 400° C. The deposition rate of tungsten may be improved by increasing the deposition temperature to, for example, about 500° C. to about 550° C. However, temperatures in this higher range may compromise the structural and operational integrity of the underlying portions of the integrated circuit being formed. Use of tungsten has also frustrated photolithography steps during the manufacturing process as it results in a relatively rough surface having a reflectivity of 70% or less than that of silicon (thickness and wavelength dependent). Further, tungsten has proven difficult to deposit uniformly. Poor surface uniformity typically increases film resistivity.
Therefore, there is a need for an improved technique to deposit conductive layers with good uniformity using cyclical deposition techniques.
In one embodiment of the invention, a method for forming a tungsten-containing layer on a substrate is provided which includes positioning a substrate containing a barrier layer disposed thereon in a process chamber, exposing the substrate to a first soak process for a first time period and depositing a nucleation layer on the barrier layer by flowing a tungsten-containing precursor and a reductant into the process chamber. The method further includes exposing the nucleation layer to a second soak process for a second time period and depositing a bulk layer on the nucleation layer. In one example, the barrier layer contains titanium nitride, the first and second soak processes independently comprise at least one reducing gas selected from the group consisting of hydrogen, silane, disilane, dichlorosilane, borane, diborane, derivatives thereof and combinations thereof and the nucleation layer may be deposited by an atomic layer deposition process or a pulsed chemical vapor deposition process while the bulk layer may be deposited by a chemical vapor deposition process or a physical vapor deposition process.
In another example of the invention, a method for forming a tungsten-containing layer on a substrate is provided which includes positioning a substrate containing a barrier layer disposed thereon in a process chamber and exposing the substrate to a first reductant to form a first treated surface on the barrier layer. The method further includes depositing a nucleation layer on the treated surface by a vapor deposition process, exposing the substrate to a second reductant to form a second treated surface, and depositing a bulk layer on the second treated surface.
In another example of the invention, a method for forming a tungsten-containing layer on a substrate is provided which includes positioning a substrate in a process chamber, depositing a nucleation layer on the substrate by a vapor deposition process, exposing the nucleation layer to a second soak process to form a treated surface, and depositing a bulk layer on the second treated surface.
In another example of the invention, a method for forming a tungsten-containing layer on a substrate is provided which includes positioning a substrate containing a barrier layer disposed thereon in a process chamber, exposing the substrate to a first soak process and depositing a nucleation layer on the barrier layer by a pulsed chemical vapor deposition process or an atomic layer deposition process. The method further includes exposing the nucleation layer to a second soak process and depositing a bulk layer on the nucleation layer by a chemical vapor deposition process or a physical vapor deposition process.
So that the manner in which the above recited features of the invention can be understood in detail, a more particular description of the invention, briefly summarized above, may be had by reference to embodiments, some of which are illustrated in the appended drawings. It is to be noted, however, that the appended drawings illustrate only typical embodiments of the invention and are therefore not to be considered limiting of its scope, for the invention may admit to other equally effective embodiments.
Embodiments of the invention provide an improved process for depositing tungsten-containing films. The process utilizes soak processes and vapor deposition processes, such as an atomic layer deposition (ALD) or pulsed-CVD to provide tungsten films having significantly improved surface uniformity and production level throughput. In one aspect, the process includes at least one soak process prior to tungsten deposition to activate the underlying surface on the substrate. Preferably, the underlying surface is exposed to a reductant, such as diborane (B2H6) or silane (SiH4), although it is believed that other reductant will achieve similar results. In general, the soak process may occur in-situ for a period of time in a range from about 1 second to about 90 seconds at similar processing conditions as a subsequent tungsten deposition process, thereby significantly increasing production throughput. For example, a soak process may be conducted to the barrier layer prior to depositing a nucleation layer thereon and/or a soak process may be conducted to the nucleation layer prior to depositing a bulk layer thereon.
A “substrate surface”, as used herein, refers to any substrate or material surface formed on a substrate upon which film processing is performed. For example, a substrate surface on which processing can be performed include materials such as silicon, silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Barrier layers, metals or metal nitrides on a substrate surface include titanium, titanium nitride, tungsten nitride, tantalum and tantalum nitride. A substrate surface may also include dielectric materials such as silicon dioxide and carbon doped silicon oxides. Substrates may have various dimensions, such as 200 mm or 300 mm diameter wafers, as well as, rectangular or square panes.
“Atomic layer deposition” or “cyclical deposition” as used herein refers to the sequential introduction of two or more reactive compounds to deposit a layer of material on a substrate surface. The two or more reactive compounds are alternatively introduced into a reaction zone of a processing chamber. Each reactive compound is separated by a time delay to allow each compound to adhere and/or react on the substrate surface. In one aspect, a first precursor or compound A is pulsed into the reaction zone followed by a first time delay. Next, a second precursor or compound B is pulsed into the reaction zone followed by a second delay. During each time delay a purge gas, such as argon, is introduced into the processing chamber to purge the reaction zone or otherwise remove any residual reactive compound or by-products from the reaction zone. Alternatively, the purge gas may flow continuously throughout the deposition process so that only the purge gas flows during the time delay between pulses of reactive compounds. The reactive compounds are alternatively pulsed until a desired film or film thickness is formed on the substrate surface. In either scenario, the ALD process of pulsing compound A, purge gas, compound B and purge gas is a cycle. A cycle can start with either compound A or compound B and continue the respective order of the cycle until achieving a film with the desired thickness.
Suitable carrier gases or purge gases include helium, argon, nitrogen, hydrogen, forming gas and combinations thereof. Typically, the borane compounds utilize argon or nitrogen as a carrier gas and the silane compounds use hydrogen, argon or nitrogen as the carrier gas.
A “pulse” as used herein is intended to refer to a quantity of a particular compound that is intermittently or non-continuously introduced into a reaction zone of a processing chamber. The quantity of a particular compound within each pulse may vary over time, depending on the duration of the pulse. The duration of each pulse is variable depending upon a number of factors such as, for example, the volume capacity of the process chamber employed, the vacuum system coupled thereto, and the volatility/reactivity of the particular compound itself.
Referring to step 170, after each deposition cycle (steps 130 through 160), a tungsten nucleation layer having a particular thickness will be deposited on the substrate surface. Usually, each deposition cycle forms a layer with a thickness in the range from about 1 Å to about 10 Å. Depending on specific device requirements, subsequent deposition cycles may be needed to deposit tungsten nucleation layer having a desired thickness. As such, a deposition cycle (steps 130 through 160) can be repeated until the desired thickness for the tungsten film is achieved. The nucleation layer is typically deposited to a thickness in a range from about 10 Å to about 200 Å. Thereafter, the process is stopped as indicated by step 180 when the desired thickness is achieved.
Suitable tungsten-containing precursors or compounds include tungsten hexafluoride (WF6), tungsten hexachloride (WCl6), tungsten carbonyl (W(CO)6), bis(cyclopentadienyl)tungsten dichloride (Cp2WCl2) and mesitylene tungsten tricarbonyl (C9H12W(CO)3), as well as derivatives thereof. Suitable reducing compounds and soak compounds include silane compounds, borane compounds, phosphine compounds, ammonia and ammine compounds and hydrogen. Silane compounds include silane, disilane, trisilane, tetrasilane, chlorosilane, dichlorosilane, tetrachlorosilane, hexachlorodisilane and derivatives thereof, while borane compounds include borane, diborane, triborane, tetraborane, pentaborane, alkylboranes, such as triethylborane and derivatives thereof. The preferred reducing compounds and reductant for the soak process include silane, disilane, diborane, hydrogen and combinations thereof.
The substrate surface generally contains a barrier layer disposed thereon. The tungsten nucleation layer is deposited on the barrier layers. The substrate surface is exposed to a soak process at a temperature in the range from about 100° C. to about 600° C., preferably in the range from about 100° C. to about 500° C., more preferably in the range from about 300° C. to about 450° C. In one example, the temperature of the soak process is maintained for the subsequent vapor deposition process. The soak process (step 120) is typically performed with the process chamber at a pressure in the range from about 1 Torr to about 150 Torr, preferably in the range from about 5 Torr to about 90 Torr. In some examples, a pressure is in a range from about 5 Torr to about 20 Torr. In another example, the pressure is about 40 Torr. The soak process is usually conducted to the substrate surface for a time period in the range from about 1 second to about 90 seconds. In one example, the soak process will last for about 60 seconds or less. In another example, the soak process will last for about 30 seconds or less. In another aspect, the soak process will last for about 10 seconds. The soak process includes a soak compound, such as a reductant and usually has a carrier gas. The flow rate of the reductant is generally in the range from about 10 sccm to about 2,000 sccm, preferably in the range from about 50 sccm to about 500 sccm. The flow rate of the carrier gas is generally in the range from about 10 sccm to about 2,000 sccm, preferably in the range from about 50 sccm to about 500 sccm.
The barrier layer disposed on the substrate is reduced and/or adsorbs the reductant to form a conditioned layer for the subsequent nucleation layer. The conditioned barrier layer provides for a quicker and smoother deposition of the nucleation layer. In one example, diborane is introduced with hydrogen, each having a flow rate in a range from about 50 sccm to about 500 sccm. Preferably, the diborane and hydrogen gases are introduced in a 1:1 volumetric ratio. In another example, silane is introduced with hydrogen, each having a flow rate in a range from about 50 sccm to about 500 sccm. Preferably in step 120, the reductant or soak compound utilized in the soak process is diborane or silane.
In step 130, the tungsten-containing precursor is preferably tungsten hexafluoride and introduced at a rate in the range from about 5 sccm to about 200 sccm. The tungsten-containing precursor can be introduced with a carrier gas, such as argon with a flow rate in the range from about 50 sccm to about 1,000 sccm. In step 150, the reductant is preferably diborane or silane and introduced at a rate in the range from about 5 scorn to about 2,000 sccm, preferably in the range from about 50 scorn to about 500 sccm. The reductant can be introduced with a carrier gas, such as hydrogen, with a flow rate in the range from about 50 sccm to about 2,000 sccm. The pulses of a purge gas, preferably argon or nitrogen, at steps 140 and 160, are typically introduced at a rate from about 50 sccm to about 2,000 sccm, preferably at about 500 sccm. Steps 140 and 160 may include a continuous flow of purge gas whereas the tungsten-containing compound and the reducing gas are pulsed into a steady stream of carrier gas. Each processing step (steps 130 through 160) lasts from about 0.01 seconds to about 10 seconds, preferably in the range from about 0.1 seconds to about 1 second. Longer processing steps, such as about 30 seconds or about 60 seconds, achieve tungsten deposition. However, the throughput is reduced. The specific pressures and times are obtained through experimentation. In one example, a 300 mm diameter wafer needs about twice the flow rate as a 200 mm diameter wafer in order to maintain similar throughput.
An ALD process chamber used during embodiments described herein is available from Applied Materials, Inc. located in Santa Clara, Cali. A more detailed description of an ALD process chamber may be found in commonly assigned U.S. Ser. No. 10/032,284, filed on Dec. 21, 2001, and issued as U.S. Pat. No. 6,916,398, U.S. Ser. No. 10/281,079, filed on Oct. 25, 2002, and published as US 2003-0121608, and U.S. Ser. No. 10/016,300, filed on Dec. 12, 2001, and issued as U.S. Pat. No. 6,878,206, which are hereby incorporated by reference in their entirety. Software routines are executed to initiate process recipes or sequences. The software routines, when executed, transform the general purpose computer into a specific process computer that controls the chamber operation so that a chamber process is performed. For example, software routines may be used to precisely control the activation of the electronic control valves for the execution of process sequences according to aspects of the invention. Alternatively, the software routines may be performed in hardware, as an application specific integrated circuit or other type of hardware implementation, or a combination of software or hardware.
During step 210, the substrate is positioned into the process chamber. The substrate surface may contain a barrier layer disposed thereon. Barrier layers usually contain a metal or metal nitride material that includes titanium, titanium nitride, titanium silicon nitride, tantalum, tantalum nitride, tantalum silicon nitride, and combinations thereof. A barrier layer may be formed by process techniques such as chemical vapor deposition (CVD), atomic layer deposition (ALD), physical vapor deposition (PVD), derivatives thereof and combinations thereof. The barrier layer is usually deposited to a thickness of at least about 30 Å, such as in a range from about 30 Å to about 100 Å. In one example, a barrier layer is deposited on the substrate surface by a CVD process by using tetrakis(dimethylamino)titanium (TDMAT) and ammonia. In another example, a barrier layer is deposited on the substrate surface by an ALD process by sequentially pulsing titanium tetrachloride (TiCl4) and ammonia. In another example, a barrier layer is deposited on the substrate surface by a PVD process by sputtering from a titanium source in a nitrogen environment. The barrier layer may be plasma densified prior to performing a subsequent fabrication process.
The process conditions, such as temperature and pressure, set during step 210 may be used during step 220. The process chamber is adjusted to heat the substrate at a temperature in the range from about 100° C. to about 600° C., preferably in the range from about 200° C. to about 500° C., and more preferably in the range from about 300° C. to about 450° C. The process chamber is maintained at a pressure in the range from about 1 Torr to about 150 Torr, preferably in the range from about 5 Torr to about 90 Torr. In one example, the process chamber used during the soak process may be the same process chamber as used to deposit the barrier layer. In another example, the process chamber used during the soak process is used to deposit the subsequent nucleation layer during step 230.
During step 220, the substrate surface is exposed to a soak process containing a reductant and an optional carrier gas. The reductant adsorbs and/or reacts to the substrate surface, namely the barrier layer, to form a treated surface. The treated surface provides a quicker deposition process for an overall smooth and more uniform tungsten layer. The reductants may include silane compounds, borane compounds, phosphine compounds, ammonia and ammine compounds and hydrogen. Silane compounds include silane, disilane, trisilane, tetrasilane, chlorosilane, dichlorosilane, tetrachlorosilane, hexachlorodisilane and derivatives thereof, while borane compounds include borane, diborane, triborane, tetraborane, pentaborane, alkylboranes, such as triethylborane and derivatives thereof. The preferred reductants include silane, disilane, diborane and hydrogen. A carrier gas may be co-flowed with the reductant. Carrier gases include hydrogen, nitrogen, argon, helium and combinations thereof. For example, diborane is often used with a concentration of 5 vol % in argon or nitrogen.
The soak process in step 220 usually last for a period of time in the range from about 1 second to about 90 seconds. The barrier layer disposed on the substrate is reduced and/or adsorbs the reductant to form a conditioned layer for the subsequent nucleation layer. In one example performed prior to an ALD nucleation process, about 300 sccm of a 5 vol % diborane in argon is exposed to the substrate for about 30 seconds at about 15 Torr and about 350° C. In one example performed prior to a pulsed-CVD nucleation process, about 200 sccm of a 5 vol % diborane in nitrogen is exposed to the substrate for about 24 seconds at about 90 Torr and about 400° C.
During step 230, a nucleation layer is deposited on the substrate surface, namely on the treated barrier layer. The nucleation layer may be deposited by a vapor deposition process that includes ALD, CVD and/or pulsed-CVD. The process chamber used to deposit the nucleation layer may be the same process chamber used in the soak processes as described in steps 220 and 240. The nucleation layer may comprise tungsten, tungsten alloys, tungsten-containing materials (e.g., tungsten boride or tungsten silicide) and combinations thereof. The nucleation layer is typically deposited to a thickness in a range from about 10 Å to about 200 Å. In one example, an ALD process utilizing WF6 and B2H6 deposits a nucleation layer with a thickness in a range from about 10 Å to about 20 Å, such as about 12 Å. In another example, an ALD process utilizing WF6 and SiH4 deposits a nucleation layer with a thickness in a range from about 10 Å to about 50 Å, such as about 30 Å. In another example, a pulsed-CVD (e.g., co-flowed) process utilizing WF6 and SiH4 or WF6 and B2H6 deposits a nucleation layer with a thickness in a range from about 30 Å to about 200 Å, such as about 50 Å. Preferably, the ALD process as described herein during process 100 may be used to deposit the nucleation layer.
During step 240, the substrate surface is exposed to a post soak process or a second soak process containing a reductant and an optional carrier gas. The reductant adsorbs and/or reacts to the substrate surface, namely the nucleation layer, to form a treated surface. The reductants, as described above, may also include silane compounds, borane compounds, phosphine compounds, ammonia and ammine compounds and hydrogen. The preferred reductants include silane, disilane, diborane and hydrogen. A carrier gas may be co-flowed with the reductant and include hydrogen, nitrogen, argon, helium and combinations thereof. For example, diborane is often used with a concentration of 5 vol % in argon or nitrogen.
The soak process in step 240 usually last for a period of time in the range from about 1 second to about 90 seconds. The process chamber is adjusted to heat the substrate at a temperature in the range from about 100° C. to about 600° C., preferably in the range from about 200° C. to about 500° C., more preferably in the range from about 300° C. to about 450° C. The process chamber is maintained at a pressure in the range from about 1 Torr to about 150 Torr, preferably in the range from about 5 Torr to about 90 Torr. The barrier layer disposed on the substrate is reduced and/or adsorbs the reductant to form a conditioned layer for the subsequent bulk layer. In one example performed after an ALD nucleation process, about 300 sccm of a 5 vol % diborane in nitrogen is exposed to the substrate for about 30 seconds at about 30 Torr and about 300° C. In one example performed after a pulsed-CVD nucleation process, about 200 sccm of a 5 vol % diborane in argon is exposed to the substrate for about 30 seconds at about 15 Torr and about 400° C. In another example performed after a pulsed-CVD nucleation process, about 300 sccm of a 5 vol % diborane in argon is exposed to the substrate for about 10 seconds at about 90 Torr and about 400° C.
During step 250, a bulk layer is deposited on the substrate surface, namely on the treated nucleation layer. The bulk layer may be deposited by a vapor deposition process that includes CVD, pulsed-CVD and/or PVD. The process chamber used to deposit the bulk layer may be the same process chamber used in the post soak process as described in step 240. The bulk layer comprises tungsten, tungsten alloys, tungsten-containing materials (e.g., tungsten boride, tungsten silicide or tungsten phosphide) and combinations thereof. The bulk layer is typically deposited to a thickness in the range from about 100 Å to about 10,000 Å, preferably from about 1,000 Å to about 5,000 Å. In one example, a CVD process utilizing WF6 and B2H6 is used to deposit a bulk layer on the treated nucleation layer. In another example, a CVD process utilizing WF6 and SiH4 is used to deposit a bulk layer on the treated nucleation layer. In another example, a PVD process utilizing a tungsten source is used to deposit a bulk layer on the treated nucleation layer. Processes for soaking a tungsten nucleation layer and depositing a tungsten bulk layer thereon is further described in the commonly assigned U.S. Pat. No. 6,156,382, which is incorporated by reference herein.
In an alternative embodiment, a tungsten-containing film is deposited by depositing more than one nucleation layer and may include multiple cycles of a vapor deposition process. In one example, the barrier layer may be exposed to a soak process prior to forming a first nucleation layer by a pulsed-CVD process. The process chamber is heated to a temperature in a range from about 400° C. to about 450° C., for example, about 425° C. and maintained at a pressure in a range from about 10 Torr to about 20 Torr, such as about 15 Torr. The pulsed-CVD process may include exposing the substrate to a co-flow of a tungsten-containing compound and a reductant for a period of time from about 1 second to about 3 seconds, for example about 1.5 seconds. The flow of the reagents include the tungsten-containing compound with a flow rate from about 30 sccm to about 90 sccm, such as about 60 sccm, while the reductant is at a flow rate from about 10 sccm to about 50 sccm, such as about 30 sccm. The co-flow is stopped and the process chamber purged. Then the reductant is pulsed into the chamber for a period of time from about 1 second to about 3 seconds, for example about 1 second. The reductant may have a flow rate from about 10 sccm to about 50 sccm, such as about 30 sccm. The flow of the reductant is stopped and the chamber purged for about 0.5 seconds. The cycle is repeated until a predetermined thickness of the first nucleation layer is formed. For example, the process is repeated 3 times to form a layer with a thickness about 30 Å. The preferred tungsten-containing compound is tungsten hexafluoride and the preferred reductant is silane and/or diborane. The reductant is optionally used during a soak process prior or subsequent the deposition of the first nucleation layer.
A second nucleation layer may be formed on the first nucleation layer. The process chamber may be kept at the same temperature, but the pressure of the process chamber is usually increased. The process chamber is maintained at a temperature in a range from about 400° C. to about 450° C., for example, about 425° C. and the a pressure is in a range from about 20 Torr to about 50 Torr, such as about 30 Torr. The CVD process may include exposing the substrate to a co-flow of a tungsten-containing compound and a reductant for a period of time from about 4 seconds to about 8 seconds, for example about 6 seconds. The flow of the reagents include the tungsten-containing compound with a flow rate from about 30 sccm to about 70 sccm, such as about 50 sccm, while the reductant has a flow rate from about 10 sccm to about 50 sccm, such as about 25 sccm. A second nucleation layer is deposited on the first nucleation layer and has a thickness in a range from about 50 Å to about 1,000 Å, preferably from about 150 Å to about 300 Å. The preferred tungsten-containing compound is tungsten hexafluoride and the preferred reductant is silane and/or diborane. The reductant is optionally used during a soak process prior or subsequent the deposition of the second nucleation layer.
Finally, a bulk layer may be deposited on the second nucleation layer. The bulk layer may be deposited by a tradition CVD process. In one example, the process chamber is maintained at a temperature in a range from about 400° C. to about 450° C., for example, about 425° C. and the pressure is maintained in a range from about 100 Torr to about 350 Torr, such as about 200 Torr. The flow of the reagents include the tungsten-containing compound with a flow rate from about 200 sccm to about 800 sccm, such as about 400 sccm, while the reductant has a flow rate from about 2,000 sccm to about 8,000 sccm, such as about 4,000 sccm. The preferred tungsten-containing compound is tungsten hexafluoride and the preferred reductant is hydrogen.
Process Integration
A tungsten nucleation layer as described above has shown particular utility when integrated with traditional bulk fill techniques to form features with excellent film properties. An integration scheme can include ALD or pulsed-CVD processes to deposit a nucleation layer while a bulk layer may be deposited by CVD or PVD processes. Integrated processing systems capable of performing such an integration scheme include an Endura®, Endura SL®, Centura® and Producer® processing systems, each available from Applied Materials, Inc. located in Santa Clara, Calif. Any of these systems can be configured to include at least one ALD or pulsed-CVD chamber for depositing the nucleation layer and at least one CVD chamber or PVD chamber for bulk fill.
The transfer chambers 322, 324, are used to maintain ultrahigh vacuum conditions while allowing substrates to be transferred within the system 300. A second robot 330 may transfer the substrates between the transfer chambers 322, 324 and a second set of one or more processing chambers 332, 334, 336, 338. Similar to processing chambers 312, 314, 316, 318, the processing chambers 332, 334, 336, 338 can be outfitted to perform a variety of substrate processing operations, such as cyclical deposition, CVD, PVD, etch, pre-clean, de-gas, and orientation, for example. Any of the substrate processing chambers 312, 314, 316, 318, 332, 334, 336, 338 may be removed from the system 300 if not necessary for a particular process to be performed by the system 300.
In one arrangement, each processing chamber 332 and 338 may be a cyclical deposition chamber adapted to deposit a nucleation layer; each processing chamber 334 and 336 may be a cyclical deposition chamber, a chemical vapor deposition chamber or a physical vapor deposition chamber adapted to form a bulk layer; each processing chamber 312 and 314 may be a physical vapor deposition chamber, a chemical vapor deposition chamber, or a cyclical deposition chamber adapted to deposit a dielectric layer; and each processing chamber 316 and 318 may be an etch chamber outfitted to etch apertures or openings for interconnect features. This one particular arrangement of the system 300 is provided to illustrate the invention and should not be used to limit the scope of the invention.
Another integrated system may include nucleation deposition as well as bulk fill deposition in a single chamber. A chamber configured to operate in both a cyclical deposition mode as well as a conventional CVD mode can be used. One example of such a chamber is described in commonly assigned U.S. Ser. No. 10/016,300, filed on Dec. 12, 2001, and issued as U.S. Pat. No. 6,878,206, which is incorporated herein by reference.
In another integration scheme, one or more cyclical deposition nucleation chambers are integrated onto a first processing system while one or more bulk layer deposition chambers are integrated onto a second processing system. In this configuration, substrates are first processed in the first system where a nucleation layer is deposited on a substrate. Thereafter, the substrates are moved to the second processing system where bulk deposition occurs.
In one arrangement, each processing chamber 364 and 370 may be a cyclical deposition chamber adapted to deposit a nucleation layer; each processing chamber 366 and 368 may be a cyclical deposition chamber, a chemical vapor deposition chamber or a physical vapor deposition chamber adapted to form a bulk fill deposition layer. This one particular arrangement of the system 350 is provided to illustrate the invention and should not be used to limit the scope of the invention.
Alternatively, a carousel type batch processing system having a plurality of stations in a single chamber can be adapted to incorporate nucleation and bulk layer deposition into a single processing system. In such a processing system a purge gas curtain, such as an argon gas curtain, can be established between each station creating a micro or mini environment at each station. The substrates are loaded into the system sequentially and then rotated through each station and processed at least partially at each station. For example, a substrate may be exposed to a cyclical deposition nucleation step at a first station and then to partial bulk fill CVD steps at each of the subsequent stations. Alternatively, nucleation may occur at more than one station and bulk fill may occur at one or more stations. Still further, the nucleation layer and the bulk layer may be deposited in separate carousel type systems. In another aspect, the soak and the nucleation steps are completed in one carousel while the bulk steps are done on another carousel, wherein both carousels are part of the same process system. Each platen can be temperature controlled to provide at least some process control at each station. However, the process pressure typically remains the same between stations because the stations are housed in a single chamber. Some pressure control may be available in a micro or mini environment present at each station due to the inert gas curtain.
Regardless of the integration scheme, the nucleation layer is typically deposited to a thickness in a range from about 10 Å to about 200 Å and the bulk layer has a thickness in a range from about 100 Å to about 10,000 Å, preferably in the range from about 1,000 Å to about 5,000 Å. However, the thickness of these films can vary depending on the feature sizes and aspect ratios of a given application. Accordingly, the films are suitably sized to accommodate the geometries of a given application. The following are some exemplary geometries and applications that can benefit from a nucleation layer deposited according to embodiments described herein. The following descriptions are intended for illustrative purposes only, and are not intended to limit the uses of the present invention.
Tungsten Metal Gate
The metal gate 410 includes an oxide layer 411, a polysilicon layer 414, a titanium nitride barrier layer 415 and a tungsten layer 422. The oxide layer 411 separates the substrate 412 from the polysilicon layer 414. The oxide layer 411 and the polysilicon layer 414 are deposited using conventional deposition techniques.
The titanium nitride barrier layer 415 is deposited on the polysilicon layer 414. The titanium nitride barrier layer 415 may be a bi-layer stack formed by depositing a PVD titanium layer followed by a CVD titanium nitride layer. The titanium nitride barrier layer 415 may also be deposited using a cyclical deposition technique, such as the process shown and described in commonly assigned U.S. Ser. No. 10/032,293, filed on Dec. 21, 2001, entitled “Chamber Hardware Design for Titanium Nitride Atomic Layer Deposition,” published as U.S. Patent Publication 20030116087, which is incorporated by reference herein.
A soak process is administered to the substrate surface. The soak includes a silane compound or a borane compound along with at least one carrier gas. A preferred silane compound is silane, a preferred borane compound is diborane and a preferred carrier gas is either hydrogen, nitrogen and/or argon. In one aspect, silane has a flow rate in the range from about 25 sccm to about 500 sccm and hydrogen has a flow rate in the range from about 200 sccm to about 700 sccm. The soak process is conducted at a temperature in the range from about 100° C. to about 500° C., preferably at about 300° C., a pressure in the range from about 1 Torr to about 150 Torr, preferably from about 30 Torr to about 120 Torr and for a time period from about 1 second to about 90 seconds. In another aspect, diborane has a flow rate in the range from about 25 sccm to about 500 sccm and hydrogen and/or argon has a flow rate in the range from about 200 sccm to about 700 sccm. The soak process is conducted at a temperature in the range from about 100° C. to about 500° C., preferably at about 300° C., a pressure in the range from about 1 Torr to about 120 Torr, preferably at about 5 Torr to about 50 Torr, and a period of time from about 1 second to about 90 seconds, preferably less than about 60 seconds.
In one example, a nucleation layer 417 is then cyclically deposited over the barrier layer 415 following treatment of the substrate surface with a soak process. In one aspect, the nucleation layer 417 is cyclically deposited using alternating pulses of tungsten hexafluoride and diborane. The tungsten hexafluoride is pulsed at a rate of between about 1 sccm and about 100 sccm, such as between about 5 sccm and about 50 sccm, for about 0.3 seconds. A carrier gas, such as argon, is provided along with the tungsten hexafluoride at a rate of about 100 sccm to about 1,000 sccm, such as between about 100 sccm to about 500 sccm. The diborane is pulsed at a rate of about 50 sccm and about 1,000 sccm, such as between about 400 sccm and about 600 sccm, for about 0.3 seconds. A carrier gas, such as hydrogen, is provided along with the diborane at a rate between about 50 sccm to about 500 sccm, such as between about 100 sccm to about 300 sccm. The substrate is maintained at a temperature between about 100° C. and about 400° C., preferably at about 300° C., at a chamber pressure between about 1 Torr and about 120 Torr, preferably between about 5 Torr and about 50 Torr. In between pulses of the tungsten hexafluoride and the diborane, argon is pulsed for about 0.5 seconds to purge or otherwise remove any reactive compounds from the processing chamber.
In another aspect, the nucleation layer 417 is cyclically deposited using alternating pulses of tungsten hexafluoride and silane. The tungsten hexafluoride is pulsed as described above with argon for about 0.5 seconds. The silane is pulsed at a rate of about 1 sccm to about 100 sccm, such as between about 5 sccm to about 50 sccm, for about 0.5 seconds. A carrier gas, such as hydrogen, is provided along with the silane at a rate of about 100 sccm and about 1,000 sccm, such as between about 100 sccm and about 500 sccm. Argon is pulsed at a rate of about 100 sccm to about 1,000 sccm, such as between about 300 sccm to about 700 sccm, for about 0.5 seconds between the pulses of the tungsten hexafluoride and the pulses of silane. The substrate is maintained at a temperature between about 100° C. and about 400° C., preferably at about 300° C., at a chamber pressure between about 1 Torr and about 30 Torr.
In another example, a nucleation layer 417 is deposited by a pulsed-CVD process on the barrier layer 415 following treatment of the substrate surface with a soak process. The pulsed-CVD process includes co-flowing WF6 and B2H6 or WF6 and SiH4 at a temperature in a range from about 300° C. to about 500° C., preferably from about 400° C. to about 450° C. The pulsed-CVD process pulses the co-flowing precursors at a time period from about 0.5 seconds to about 3 seconds, preferably about 1.5.
A second soak process or post soak process is administered to the substrate surface. The soak process includes a reductant, such as silane compound or a borane compound along with at least one carrier gas. Preferably, the reductant is diborane and a preferred carrier gas is hydrogen, nitrogen and/or argon. In one example, a reducing gas containing 5 vol % of diborane in argon has a flow rate in the range from about 100 sccm to about 500 sccm, preferably about 300 sccm. The soak process is conducted at a temperature in the range from about 100° C. to about 500° C., preferably about 300° C., a pressure in the range from about 1 Torr to about 120 Torr, preferably at about 10 Torr to about 50 Torr, and for a time period from about 1 second to about 90 seconds, preferably less than about 30 seconds.
A nucleation layer formed utilizing soak processes has advantages over a nucleation layer formed without the soak processes. The tungsten film shows less stress for the integrated film, as well as, less fluorine content at the interface of the nucleation layer. Also, the nucleation layer deposited post a soak treatment has higher uniformity coverage and is deposited quicker due to a reduced incubation period.
A tungsten bulk fill 422 is then deposited on the treated tungsten nucleation layer 417. Although any metal deposition process, such as conventional chemical vapor deposition or physical vapor deposition, may be used, the tungsten bulk fill 422 may be deposited by alternately adsorbing a tungsten-containing compound and a reducing compound as described above. A more detailed description of tungsten deposition using a cyclical deposition technique may be found in commonly assigned U.S. Ser. No. 10/016,300, filed on Dec. 12, 2001, and issued as U.S. Pat. No. 6,878,206 and in commonly assigned U.S. Ser. No. 10/082,048, filed on Feb. 20, 2002, and published as US 2003-0157760, which are both incorporated herein by reference. Fewer volcanoes appear on the surface of the tungsten film deposited utilizing a soak process, as compared to tungsten films deposited without exploiting a soak process, post tungsten bulk-fill.
Following deposition, the top portion of the resulting structure 400 may be planarized. A chemical mechanical polishing (CMP) apparatus may be used, such as the Mirra™ System available from Applied Materials, Santa Clara, Calif., for example. Portions of the tungsten bulk fill 422 are removed from the top of the structure leaving a fully planar surface. Optionally, the intermediate surfaces of the structure may be planarized between the depositions of the subsequent layers described above.
The source and drain regions 522, 524 may be connected to a tungsten plug 560. Each tungsten plug 560 includes a titanium liner 562, a tungsten nucleation layer 564, and a bulk tungsten fill 566. The titanium liner 562 may be a bi-layer stack comprising PVD titanium followed by CVD titanium nitride. Alternatively, the titanium liner 562 may be a bi-layer stack comprising ALD deposited titanium followed by ALD deposited titanium nitride. The tungsten nucleation layer 564 is formed by using a soak process and an ALD process or a soak process and a pulsed-CVD process as described above. The tungsten bulk fill 566 may be deposited using a post soak process and any conventional deposition techniques, including ALD, CVD and PVD.
The trench capacitor 530 generally includes a first electrode 532, a second electrode 534 and a dielectric material 536 disposed therebetween. The P+ substrate serves as a first electrode 532 of the trench capacitor 530 and is connected to a ground connection 541. A trench 538 is formed in the P+ substrate and filled with a heavily doped N+ polysilicon that serves as the second electrode 534 of the trench capacitor 530. The dielectric material 536 is disposed between the first electrode 532 (i.e., P+ substrate) and the second electrode 534 (i.e., N+ polysilicon).
The trench capacitor 530 also includes a first tungsten nitride barrier layer 540 disposed between the dielectric material 536 and the first electrode 532. Preferably, a second tungsten nitride barrier layer 542 is disposed between the dielectric material 536 and the second electrode 534. Alternatively, the barrier layers 540, 542 are a combination film, such as W/WN.
Although the above-described DRAM device utilizes an n-p-n transistor, a P+ substrate as a first electrode, and an N+ polysilicon as a second electrode of the capacitor, other transistor designs and electrode materials are contemplated by the present invention to form DRAM devices. Additionally, other devices, such as crown capacitors for example, are contemplated by the present invention.
The following examples were conducted to substrates that contained a barrier layer deposited on the surface. The barrier layer was formed by first depositing a titanium layer by a PVD process on a 300 mm substrate surface to a thickness of about 20 Å. Subsequently, a titanium nitride layer was deposited on the titanium layer using a CVD process of co-flowing PDMAT and ammonia. The tantalum nitride layer was deposited to a thickness of about 80 Å.
The substrate was placed into an ALD chamber and exposed to a soak process under the following conditions:
Next, a tungsten nucleation layer was formed on the barrier layer in the same ALD chamber from the previous soak process using an ALD process under the following conditions:
The cycle was repeated 4 times to form a nucleation layer with a thickness of about 12 Å. Thereafter, the substrate was maintained in the ALD chamber and exposed to a second soak process under the following conditions:
Finally, the substrate was transferred into a CVD chamber and a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the nucleation layer using a CVD process at about 400° C. The resulting tungsten bulk fill film exhibited a uniformity variance of less than about 2 percent.
The substrate was placed into an ALD chamber and exposed to a soak process under the following conditions:
Next, a tungsten nucleation layer was formed on the barrier layer in the same ALD chamber as used in the prior soak process using an ALD process under the following conditions:
The cycle was repeated 4 times to form a nucleation layer with a thickness of about 30 Å. Thereafter, the substrate was transferred to a CVD chamber and exposed to a second soak process under the following conditions:
Finally, the substrate was maintained in the CVD chamber and a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the nucleation layer using a CVD process at about 400° C. The resulting tungsten bulk fill film exhibited a uniformity variance of less than about 4 percent.
The substrate was placed into a CVD chamber and exposed to a soak process under the following conditions:
Next, a tungsten nucleation layer was formed on the barrier layer in the CVD chamber from the previous soak process using a pulsed-CVD process under the following conditions:
The pulsed-CVD process was continued until the nucleation layer had a thickness of about 50 Å. Thereafter, the substrate was kept in the CVD chamber and a second nucleation layer was deposited on the first nucleation layer. The second nucleation layer was deposited by a traditional CVD process to a thickness of about 200 Å under the following conditions:
Subsequently, a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the second nucleation layer using a CVD process at about 400° C.
The substrate was placed into a CVD chamber and exposed to a soak process under the following conditions:
Next, a tungsten nucleation layer was formed on the barrier layer in the previously used CVD chamber using a pulsed-CVD process under the following conditions:
The pulsed-CVD process was continued until the nucleation layer had a thickness of about 50 Å. Thereafter, the substrate was kept in the CVD chamber and a second nucleation layer was deposited on the first nucleation layer. The second nucleation layer was deposited by a traditional CVD process to a thickness of about 200 Å under the following conditions:
The substrate was placed into a CVD chamber and exposed to a soak process under the following conditions:
Next, a tungsten nucleation layer was formed on the barrier layer in the same CVD chamber used during the soak process using a pulsed-CVD process under the following conditions:
The pulsed-CVD process was continued until the nucleation layer had a thickness of about 150 Å. Thereafter, the substrate was kept in the CVD chamber and exposed to a second soak process under the following conditions:
Finally, the substrate was maintained in the CVD chamber and a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the nucleation layer using a CVD process at about 400° C. The resulting tungsten bulk fill film exhibited a uniformity variance of less than about 4 percent.
The substrate was placed into a CVD chamber and exposed to a soak process under the following conditions:
Next, a tungsten nucleation layer was formed on the barrier layer in the CVD chamber used during the prior soak process using a pulsed-CVD process under the following conditions:
The pulsed-CVD process was continued until the nucleation layer had a thickness of about 150 Å. Thereafter, the substrate was kept in the CVD chamber and exposed to a second soak process under the following conditions:
Finally, the substrate was maintained in the CVD chamber and a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the nucleation layer using a CVD process at about 400° C. The resulting tungsten bulk fill film exhibited a uniformity variance of less than about 2 percent.
The substrate was placed into a CVD chamber and exposed to a soak process under the following conditions:
Next, the soak process is stopped for 0.5 seconds, the chamber purged and then a tungsten nucleation layer was formed on the barrier layer in the CVD chamber used during the prior soak process using a pulsed-CVD process under the following conditions:
The first nucleation process was stopped and the chamber purged for about 0.5 seconds. Then the soak process and the pulsed-CVD process were repeated in a cycle for three times to form a first nucleation layer with a thickness of about 50 Å. Thereafter, the substrate was kept in the CVD chamber and exposed to a traditional CVD process to form a second nucleation layer with a thickness of about 200 Å on the first nucleation layer under the following conditions:
Finally, the substrate was maintained in the CVD chamber and a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the second nucleation layer using a CVD process under the following conditions:
The substrate was placed into a CVD chamber and exposed to a soak process under the following conditions:
Next, the soak process is stopped for 0.5 seconds, the chamber purged and then a tungsten nucleation layer was formed on the barrier layer in the CVD chamber used during the prior soak process using a pulsed-CVD process under the following conditions:
The first nucleation process was stopped and the chamber purged for about 0.5 seconds. Then the soak process and the pulsed-CVD process were repeated in a cycle for three times to form a first nucleation layer with a thickness of about 50 Å. Thereafter, the substrate was kept in the CVD chamber and exposed to a traditional CVD process to form a second nucleation layer with a thickness of about 200 Å on the first nucleation layer under the following conditions:
Finally, the substrate was maintained in the CVD chamber and a bulk tungsten layer was deposited to a thickness of about 2,500 Å on the second nucleation layer using a CVD process under the following conditions:
While the foregoing is directed to embodiments of the invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, and the scope thereof is determined by the claims that follow.
This application is a continuation-in-part of U.S. patent application Ser. No. 10/418,728, entitled “Method for Depositing Refractory Metal Layers Employing Sequential Deposition Techniques,” filed on Apr. 18, 2003, which is a continuation-in-part of U.S. patent Ser. No. 10/268,195 filed Oct. 10, 2002 now U.S. Pat. No. 6,797,340, filed Oct. 10, 2002, which claims priority to U.S. Provisional Patent Application Ser. No. 60/328,451, entitled “Method and Apparatus for Depositing Refractory Metal Layers Employing Sequential Deposition Techniques,” filed on Oct. 10, 2001, which are all hereby incorporated by reference in their entirety. This application is also a continuation-in-part of U.S. patent No. application Ser. No. 10/879,448, entitled, “Method for Depositing Refractory Metal Layers Employing Sequential Deposition Techniques,” filed Jun. 29, 2004, which is a continuation of U.S. patent Ser. No. 10/268,195 filed Oct. 10, 2002 now U.S. Pat. No. 6,797,340, filed Oct. 10, 2002, which claims priority to U.S. Provisional Patent Application Ser. No. 60/328,451, entitled “Method and Apparatus for Depositing Refractory Metal Layers Employing Sequential Deposition Techniques,” filed on Oct. 10, 2001, which are all hereby incorporated by reference in their entirety. This application is also a continuation-in-part of U.S. patent application Ser. No. 10/762,764, entitled “Method and Apparatus for Depositing Refractory Metal Layers Employing Sequential Deposition Techniques to form Nucleation Layer,” filed on Jan. 22, 2004 now abandoned, which is a continuation of U.S. patent application Ser. No. 09/678,266, entitled “Method and Apparatus for Depositing Refractory Metal Layers Employing Sequential Deposition Techniques to Form Nucleation Layer,” filed on Oct. 3, 2000, and issued as U.S. Pat. No. 7,101,795, which is a continuation-in-part of U.S. patent Ser. No. 09/605,593 filed Jun. 28, 2000 now U.S. Pat. No. 6,551,929, filed on Jun. 28, 2000, which are all hereby incorporated by reference in their entirety. This application is also a continuation-in-part of U.S. patent application Ser. No. 10/196,514, entitled “Method and Apparatus for Depositing Tungsten After Surface Treatment to Improve Film Characteristics,” filed on Jul. 15, 2002, and issued as U.S. Pat. No. 6,936,538, which claims priority to U.S. Provisional Patent Application Ser. No. 60/305,765, entitled “Method and Apparatus for Depositing Tungsten After Surface Treatment to Improve Film Characteristics,” filed on Jul. 16, 2001, which are both hereby incorporated by reference in their entirety.
Number | Name | Date | Kind |
---|---|---|---|
4058430 | Suntola et al. | Nov 1977 | A |
4389973 | Suntola et al. | Jun 1983 | A |
4413022 | Suntola et al. | Nov 1983 | A |
4486487 | Skarp | Dec 1984 | A |
4767494 | Kobayashi et al. | Aug 1988 | A |
4806321 | Nishizawa et al. | Feb 1989 | A |
4813846 | Helms | Mar 1989 | A |
4829022 | Kobayashi et al. | May 1989 | A |
4834831 | Nishizawa et al. | May 1989 | A |
4838983 | Schumaker et al. | Jun 1989 | A |
4838993 | Aoki et al. | Jun 1989 | A |
4840921 | Matsumoto | Jun 1989 | A |
4845049 | Sunakawa | Jul 1989 | A |
4859625 | Nishizawa et al. | Aug 1989 | A |
4859627 | Sunakawa | Aug 1989 | A |
4861417 | Mochizuki et al. | Aug 1989 | A |
4876218 | Pessa et al. | Oct 1989 | A |
4917556 | Stark et al. | Apr 1990 | A |
4927670 | Erbil | May 1990 | A |
4931132 | Aspnes et al. | Jun 1990 | A |
4951601 | Maydan et al. | Aug 1990 | A |
4960720 | Shimbo | Oct 1990 | A |
4975252 | Nishizawa et al. | Dec 1990 | A |
4976839 | Inoue | Dec 1990 | A |
4993357 | Scholz | Feb 1991 | A |
5000113 | Wang et al. | Mar 1991 | A |
5013683 | Petroff et al. | May 1991 | A |
5028565 | Chang et al. | Jul 1991 | A |
5082798 | Arimoto | Jan 1992 | A |
5085885 | Foley et al. | Feb 1992 | A |
5091320 | Aspnes et al. | Feb 1992 | A |
5130269 | Kitahara et al. | Jul 1992 | A |
5166092 | Mochizuki et al. | Nov 1992 | A |
5173474 | Connell et al. | Dec 1992 | A |
5186718 | Tepman et al. | Feb 1993 | A |
5205077 | Wittstock | Apr 1993 | A |
5225366 | Yoder | Jul 1993 | A |
5234561 | Randhawa et al. | Aug 1993 | A |
5246536 | Nishizawa et al. | Sep 1993 | A |
5250148 | Nishizawa et al. | Oct 1993 | A |
5254207 | Nishizawa et al. | Oct 1993 | A |
5256244 | Ackerman | Oct 1993 | A |
5259881 | Edwards et al. | Nov 1993 | A |
5270247 | Sakuma et al. | Dec 1993 | A |
5278435 | Van Hove et al. | Jan 1994 | A |
5281274 | Yoder | Jan 1994 | A |
5286296 | Sato et al. | Feb 1994 | A |
5290748 | Knuuttila et al. | Mar 1994 | A |
5294286 | Nishizawa et al. | Mar 1994 | A |
5296403 | Nishizawa et al. | Mar 1994 | A |
5300186 | Kitahara et al. | Apr 1994 | A |
5306666 | Izumi | Apr 1994 | A |
5311055 | Goodman et al. | May 1994 | A |
5316615 | Copel et al. | May 1994 | A |
5316793 | Wallace et al. | May 1994 | A |
5330610 | Eres et al. | Jul 1994 | A |
5336324 | Stall et al. | Aug 1994 | A |
5338389 | Nishizawa et al. | Aug 1994 | A |
5348911 | Jurgensen et al. | Sep 1994 | A |
5374570 | Nasu et al. | Dec 1994 | A |
5395791 | Cheng et al. | Mar 1995 | A |
5438952 | Otsuka | Aug 1995 | A |
5439876 | Graf et al. | Aug 1995 | A |
5441703 | Jurgensen | Aug 1995 | A |
5443033 | Nishizawa et al. | Aug 1995 | A |
5443647 | Aucoin et al. | Aug 1995 | A |
5455072 | Bension et al. | Oct 1995 | A |
5458084 | Thorne et al. | Oct 1995 | A |
5469806 | Mochizuki et al. | Nov 1995 | A |
5480818 | Matsumoto et al. | Jan 1996 | A |
5483919 | Yokoyama et al. | Jan 1996 | A |
5484664 | Kitahara et al. | Jan 1996 | A |
5503875 | Imai et al. | Apr 1996 | A |
5521126 | Okamura et al. | May 1996 | A |
5527733 | Nishizawa et al. | Jun 1996 | A |
5532511 | Nishizawa et al. | Jul 1996 | A |
5540783 | Eres et al. | Jul 1996 | A |
5580380 | Liu et al. | Dec 1996 | A |
5601651 | Watabe | Feb 1997 | A |
5609689 | Kato et al. | Mar 1997 | A |
5616181 | Yamamoto et al. | Apr 1997 | A |
5637530 | Gaines et al. | Jun 1997 | A |
5641984 | Aftergut et al. | Jun 1997 | A |
5644128 | Wollnik et al. | Jul 1997 | A |
5667592 | Boitnott et al. | Sep 1997 | A |
5674786 | Turner et al. | Oct 1997 | A |
5693139 | Nishizawa et al. | Dec 1997 | A |
5695564 | Imahashi | Dec 1997 | A |
5705224 | Murota et al. | Jan 1998 | A |
5707880 | Aftergut et al. | Jan 1998 | A |
5711811 | Suntola et al. | Jan 1998 | A |
5730801 | Tepman et al. | Mar 1998 | A |
5730802 | Ishizumi et al. | Mar 1998 | A |
5747113 | Tsai | May 1998 | A |
5749974 | Habuka et al. | May 1998 | A |
5788447 | Yonemitsu et al. | Aug 1998 | A |
5788799 | Steger et al. | Aug 1998 | A |
5796116 | Nakata et al. | Aug 1998 | A |
5801634 | Young et al. | Sep 1998 | A |
5804488 | Shih et al. | Sep 1998 | A |
5807792 | Ilg et al. | Sep 1998 | A |
5830270 | McKee et al. | Nov 1998 | A |
5835677 | Li et al. | Nov 1998 | A |
5851849 | Comizzoli et al. | Dec 1998 | A |
5855675 | Doering et al. | Jan 1999 | A |
5855680 | Soininen et al. | Jan 1999 | A |
5856219 | Naito et al. | Jan 1999 | A |
5858102 | Tsai | Jan 1999 | A |
5866213 | Foster et al. | Feb 1999 | A |
5866795 | Wang et al. | Feb 1999 | A |
5879459 | Gadgil et al. | Mar 1999 | A |
5882165 | Maydan et al. | Mar 1999 | A |
5882413 | Beaulieu et al. | Mar 1999 | A |
5904565 | Nguyen et al. | May 1999 | A |
5916365 | Sherman | Jun 1999 | A |
5923056 | Lee et al. | Jul 1999 | A |
5923985 | Aoki et al. | Jul 1999 | A |
5925574 | Aoki et al. | Jul 1999 | A |
5928389 | Jevtic | Jul 1999 | A |
5942040 | Kim et al. | Aug 1999 | A |
5947710 | Cooper et al. | Sep 1999 | A |
5972430 | DiMeo, Jr. et al. | Oct 1999 | A |
6001669 | Gaines et al. | Dec 1999 | A |
6015590 | Suntola et al. | Jan 2000 | A |
6025627 | Forbes et al. | Feb 2000 | A |
6036773 | Wang et al. | Mar 2000 | A |
6042652 | Hyun et al. | Mar 2000 | A |
6043177 | Falconer et al. | Mar 2000 | A |
6051286 | Zhao et al. | Apr 2000 | A |
6062798 | Muka | May 2000 | A |
6071808 | Merchant et al. | Jun 2000 | A |
6084302 | Sandhu | Jul 2000 | A |
6086677 | Umotoy et al. | Jul 2000 | A |
6110556 | Bang et al. | Aug 2000 | A |
6113771 | Landau et al. | Sep 2000 | A |
6113977 | Soininen et al. | Sep 2000 | A |
6117244 | Bang et al. | Sep 2000 | A |
6124158 | Dautartas et al. | Sep 2000 | A |
6130147 | Major et al. | Oct 2000 | A |
6139700 | Kang et al. | Oct 2000 | A |
6140237 | Chan et al. | Oct 2000 | A |
6140238 | Kitch | Oct 2000 | A |
6143659 | Leem | Nov 2000 | A |
6144060 | Park et al. | Nov 2000 | A |
6156382 | Rajagopalan et al. | Dec 2000 | A |
6158446 | Mohindra et al. | Dec 2000 | A |
6162715 | Mak et al. | Dec 2000 | A |
6174377 | Doering et al. | Jan 2001 | B1 |
6174809 | Kang et al. | Jan 2001 | B1 |
6174812 | Hsiung et al. | Jan 2001 | B1 |
6194310 | Hsu et al. | Feb 2001 | B1 |
6197683 | Kang et al. | Mar 2001 | B1 |
6200893 | Sneh | Mar 2001 | B1 |
6203613 | Gates et al. | Mar 2001 | B1 |
6206967 | Mak et al. | Mar 2001 | B1 |
6207302 | Sugiura et al. | Mar 2001 | B1 |
6207487 | Kim et al. | Mar 2001 | B1 |
6218298 | Hoinkis | Apr 2001 | B1 |
6245654 | Shih et al. | Jun 2001 | B1 |
6248605 | Harkonen et al. | Jun 2001 | B1 |
6258713 | Yu et al. | Jul 2001 | B1 |
6270572 | Kim et al. | Aug 2001 | B1 |
6271148 | Kao et al. | Aug 2001 | B1 |
6284646 | Leem | Sep 2001 | B1 |
6287965 | Kang et al. | Sep 2001 | B1 |
6291876 | Stumborg et al. | Sep 2001 | B1 |
6305314 | Sneh et al. | Oct 2001 | B1 |
6306216 | Kim et al. | Oct 2001 | B1 |
6309966 | Govindarajan et al. | Oct 2001 | B1 |
6316098 | Yitzchaik et al. | Nov 2001 | B1 |
6319826 | Chen et al. | Nov 2001 | B1 |
6333260 | Kwon et al. | Dec 2001 | B1 |
6335280 | Van der Jeugd | Jan 2002 | B1 |
6342277 | Sherman | Jan 2002 | B1 |
6355561 | Sandhu et al. | Mar 2002 | B1 |
6358829 | Yoon et al. | Mar 2002 | B2 |
6368954 | Lopatin et al. | Apr 2002 | B1 |
6369430 | Adetutu et al. | Apr 2002 | B1 |
6372598 | Kang et al. | Apr 2002 | B2 |
6391785 | Satta et al. | May 2002 | B1 |
6399491 | Jeon et al. | Jun 2002 | B2 |
6416822 | Chiang et al. | Jul 2002 | B1 |
6420189 | Lopatin | Jul 2002 | B1 |
6423619 | Grant et al. | Jul 2002 | B1 |
6426555 | Hsia | Jul 2002 | B1 |
6428859 | Chiang et al. | Aug 2002 | B1 |
6447933 | Wang et al. | Sep 2002 | B1 |
6451119 | Sneh et al. | Sep 2002 | B2 |
6451695 | Sneh | Sep 2002 | B2 |
6468924 | Lee et al. | Oct 2002 | B2 |
6475276 | Elers et al. | Nov 2002 | B1 |
6475910 | Sneh | Nov 2002 | B1 |
6482262 | Elers et al. | Nov 2002 | B1 |
6482733 | Raaijmakers et al. | Nov 2002 | B2 |
6482740 | Soininen et al. | Nov 2002 | B2 |
6498091 | Chen et al. | Dec 2002 | B1 |
6534395 | Werkhoven et al. | Mar 2003 | B2 |
6551929 | Kori et al. | Apr 2003 | B1 |
6569501 | Chiang et al. | May 2003 | B2 |
6599572 | Saanila et al. | Jul 2003 | B2 |
6607976 | Chen et al. | Aug 2003 | B2 |
6620723 | Byun et al. | Sep 2003 | B1 |
6630201 | Chiang et al. | Oct 2003 | B2 |
6635965 | Lee et al. | Oct 2003 | B1 |
6660126 | Nguyen et al. | Dec 2003 | B2 |
6686271 | Raaijmakers et al. | Feb 2004 | B2 |
6815285 | Choi et al. | Nov 2004 | B2 |
6838376 | Matsuse et al. | Jan 2005 | B2 |
6855368 | Kori et al. | Feb 2005 | B1 |
7141494 | Lee et al. | Nov 2006 | B2 |
7211144 | Lu et al. | May 2007 | B2 |
20010000866 | Sneh et al. | May 2001 | A1 |
20010002280 | Sneh | May 2001 | A1 |
20010009140 | Bondestam et al. | Jul 2001 | A1 |
20010009695 | Saanila et al. | Jul 2001 | A1 |
20010011526 | Doering et al. | Aug 2001 | A1 |
20010024387 | Raaijmakers et al. | Sep 2001 | A1 |
20010028924 | Sherman | Oct 2001 | A1 |
20010029094 | Mee-Young et al. | Oct 2001 | A1 |
20010031562 | Raaijmakers et al. | Oct 2001 | A1 |
20010034123 | Jeon et al. | Oct 2001 | A1 |
20010041250 | Werkhoven et al. | Nov 2001 | A1 |
20010042799 | Kim et al. | Nov 2001 | A1 |
20010054730 | Kim et al. | Dec 2001 | A1 |
20010054769 | Raaijmakers et al. | Dec 2001 | A1 |
20020000598 | Kang et al. | Jan 2002 | A1 |
20020004293 | Soininen et al. | Jan 2002 | A1 |
20020007790 | Park | Jan 2002 | A1 |
20020019121 | Pyo | Feb 2002 | A1 |
20020031618 | Sherman | Mar 2002 | A1 |
20020037630 | Agarwal et al. | Mar 2002 | A1 |
20020048880 | Lee | Apr 2002 | A1 |
20020052097 | Park | May 2002 | A1 |
20020055235 | Agarwal et al. | May 2002 | A1 |
20020060363 | Xi et al. | May 2002 | A1 |
20020061612 | Sandhu et al. | May 2002 | A1 |
20020068458 | Chiang et al. | Jun 2002 | A1 |
20020073924 | Chiang et al. | Jun 2002 | A1 |
20020076481 | Chiang et al. | Jun 2002 | A1 |
20020076507 | Chiang et al. | Jun 2002 | A1 |
20020076508 | Chiang et al. | Jun 2002 | A1 |
20020076837 | Hujanen et al. | Jun 2002 | A1 |
20020086111 | Byun et al. | Jul 2002 | A1 |
20020086507 | Park et al. | Jul 2002 | A1 |
20020090829 | Sandhu et al. | Jul 2002 | A1 |
20020094689 | Park | Jul 2002 | A1 |
20020104481 | Chiang et al. | Aug 2002 | A1 |
20020105055 | Buchanan et al. | Aug 2002 | A1 |
20020105088 | Yang et al. | Aug 2002 | A1 |
20020106536 | Lee et al. | Aug 2002 | A1 |
20020106846 | Seutter et al. | Aug 2002 | A1 |
20020109168 | Kim et al. | Aug 2002 | A1 |
20020117399 | Chen et al. | Aug 2002 | A1 |
20020121241 | Nguyen et al. | Sep 2002 | A1 |
20020121342 | Nguyen et al. | Sep 2002 | A1 |
20020121697 | Marsh | Sep 2002 | A1 |
20020144657 | Chiang et al. | Oct 2002 | A1 |
20020144855 | Chiang et al. | Oct 2002 | A1 |
20020146511 | Chiang et al. | Oct 2002 | A1 |
20020155722 | Satta et al. | Oct 2002 | A1 |
20020162506 | Sneh et al. | Nov 2002 | A1 |
20030013300 | Byun | Jan 2003 | A1 |
20030013320 | Kim et al. | Jan 2003 | A1 |
20030031807 | Elers et al. | Feb 2003 | A1 |
20030032281 | Werkhoven et al. | Feb 2003 | A1 |
20030049931 | Byun et al. | Mar 2003 | A1 |
20030049942 | Haukka et al. | Mar 2003 | A1 |
20030053799 | Lei | Mar 2003 | A1 |
20030054631 | Raaijmakers et al. | Mar 2003 | A1 |
20030072975 | Shero et al. | Apr 2003 | A1 |
20030082296 | Elers et al. | May 2003 | A1 |
20030082301 | Chen et al. | May 2003 | A1 |
20030104126 | Fang et al. | Jun 2003 | A1 |
20030116087 | Nguyen et al. | Jun 2003 | A1 |
20030123216 | Yoon et al. | Jul 2003 | A1 |
20030129826 | Werkhoven et al. | Jul 2003 | A1 |
20030134508 | Raaijmakers et al. | Jul 2003 | A1 |
20030143328 | Chen et al. | Jul 2003 | A1 |
20030143839 | Raaijmakers et al. | Jul 2003 | A1 |
20030153181 | Yoon et al. | Aug 2003 | A1 |
20030161952 | Wang et al. | Aug 2003 | A1 |
20030164421 | Collet et al. | Sep 2003 | A1 |
20030164423 | Courtois et al. | Sep 2003 | A1 |
20030182320 | Lai et al. | Sep 2003 | A1 |
20030186495 | Saanila et al. | Oct 2003 | A1 |
20030187256 | Berryman et al. | Oct 2003 | A1 |
20030187631 | Masushige et al. | Oct 2003 | A1 |
20030190423 | Yang et al. | Oct 2003 | A1 |
20030190804 | Glenn et al. | Oct 2003 | A1 |
20030194493 | Chang et al. | Oct 2003 | A1 |
20030194825 | Law et al. | Oct 2003 | A1 |
20030197402 | McCutcheon et al. | Oct 2003 | A1 |
20030197863 | Snelling et al. | Oct 2003 | A1 |
20030203616 | Chung et al. | Oct 2003 | A1 |
20030224217 | Byun et al. | Dec 2003 | A1 |
20040005749 | Choi et al. | Jan 2004 | A1 |
20040009307 | Koh et al. | Jan 2004 | A1 |
20040011504 | Ku et al. | Jan 2004 | A1 |
20040013577 | Ganguli et al. | Jan 2004 | A1 |
20040014315 | Lai et al. | Jan 2004 | A1 |
20040014320 | Chen et al. | Jan 2004 | A1 |
20040015300 | Ganguli et al. | Jan 2004 | A1 |
20040018304 | Chung et al. | Jan 2004 | A1 |
20040018723 | Byun et al. | Jan 2004 | A1 |
20040041320 | Hodumi | Mar 2004 | A1 |
20050006799 | Gregg et al. | Jan 2005 | A1 |
20050031786 | Lee et al. | Feb 2005 | A1 |
20050191803 | Matsuse et al. | Sep 2005 | A1 |
Number | Date | Country |
---|---|---|
196 27 017 | Jan 1997 | DE |
198 20 147 | Jul 1999 | DE |
0 344 352 | Jun 1988 | EP |
0 442 490 | Feb 1991 | EP |
0 429 270 | May 1991 | EP |
0 799 641 | Oct 1997 | EP |
1 167 567 | Jan 2002 | EP |
1 167 569 | Jan 2002 | EP |
2 626 110 | Jul 1989 | FR |
2 692 597 | Dec 1993 | FR |
2 355 727 | May 2001 | GB |
58-098917 | Jun 1983 | JP |
58-100419 | Jun 1983 | JP |
60-065712 | Apr 1985 | JP |
61-035847 | Feb 1986 | JP |
61-210623 | Sep 1986 | JP |
62-069508 | Mar 1987 | JP |
62-091495 | Apr 1987 | JP |
62-141717 | Jun 1987 | JP |
62-167297 | Jul 1987 | JP |
62-171999 | Jul 1987 | JP |
62-232919 | Oct 1987 | JP |
63-062313 | Mar 1988 | JP |
63-085098 | Apr 1988 | JP |
63-090833 | Apr 1988 | JP |
63-222420 | Sep 1988 | JP |
63-222421 | Sep 1988 | JP |
63-227007 | Sep 1988 | JP |
63-252420 | Oct 1988 | JP |
63-266814 | Nov 1988 | JP |
64-009895 | Jan 1989 | JP |
64-009896 | Jan 1989 | JP |
64-009897 | Jan 1989 | JP |
64-037832 | Feb 1989 | JP |
64-082615 | Mar 1989 | JP |
64-082617 | Mar 1989 | JP |
64-082671 | Mar 1989 | JP |
64-082676 | Mar 1989 | JP |
01-103982 | Apr 1989 | JP |
01-103996 | Apr 1989 | JP |
64-090524 | Apr 1989 | JP |
01-117017 | May 1989 | JP |
01-143221 | Jun 1989 | JP |
01-143233 | Jun 1989 | JP |
01-154511 | Jun 1989 | JP |
01-236657 | Sep 1989 | JP |
01-245512 | Sep 1989 | JP |
01-264218 | Oct 1989 | JP |
01-270593 | Oct 1989 | JP |
01-272108 | Oct 1989 | JP |
01-290221 | Nov 1989 | JP |
01-290222 | Nov 1989 | JP |
01-296673 | Nov 1989 | JP |
01-303770 | Dec 1989 | JP |
01-305894 | Dec 1989 | JP |
01-313927 | Dec 1989 | JP |
02-012814 | Jan 1990 | JP |
02-014513 | Jan 1990 | JP |
02-017634 | Jan 1990 | JP |
02-063115 | Mar 1990 | JP |
02-074029 | Mar 1990 | JP |
02-074587 | Mar 1990 | JP |
02-106822 | Apr 1990 | JP |
02-129913 | May 1990 | JP |
02-162717 | Jun 1990 | JP |
02-172895 | Jul 1990 | JP |
02-196092 | Aug 1990 | JP |
02-203517 | Aug 1990 | JP |
02-230690 | Sep 1990 | JP |
02-230722 | Sep 1990 | JP |
02-246161 | Oct 1990 | JP |
02-264491 | Oct 1990 | JP |
02-283084 | Nov 1990 | JP |
02-304916 | Dec 1990 | JP |
03-019211 | Jan 1991 | JP |
03-022569 | Jan 1991 | JP |
03-023294 | Jan 1991 | JP |
03-023299 | Jan 1991 | JP |
03-044967 | Feb 1991 | JP |
03-048421 | Mar 1991 | JP |
03-070124 | Mar 1991 | JP |
03-185716 | Aug 1991 | JP |
03-208885 | Sep 1991 | JP |
03-234025 | Oct 1991 | JP |
03-286522 | Dec 1991 | JP |
03-286531 | Dec 1991 | JP |
04-031391 | Feb 1992 | JP |
04-031396 | Feb 1992 | JP |
04-100292 | Apr 1992 | JP |
04-111418 | Apr 1992 | JP |
04-132214 | May 1992 | JP |
04-132681 | May 1992 | JP |
04-151822 | May 1992 | JP |
04-162418 | Jun 1992 | JP |
04-175299 | Jun 1992 | JP |
04-186824 | Jul 1992 | JP |
04-212411 | Aug 1992 | JP |
04-260696 | Sep 1992 | JP |
04-273120 | Sep 1992 | JP |
04-285167 | Oct 1992 | JP |
04-291916 | Oct 1992 | JP |
04-325500 | Nov 1992 | JP |
04-328874 | Nov 1992 | JP |
05-029228 | Feb 1993 | JP |
05-047665 | Feb 1993 | JP |
05-047666 | Feb 1993 | JP |
05-047668 | Feb 1993 | JP |
05-074717 | Mar 1993 | JP |
05-074724 | Mar 1993 | JP |
05-102189 | Apr 1993 | JP |
05-160152 | Jun 1993 | JP |
05-175143 | Jul 1993 | JP |
05-175145 | Jul 1993 | JP |
05-182906 | Jul 1993 | JP |
05-186295 | Jul 1993 | JP |
05-206036 | Aug 1993 | JP |
05-234899 | Sep 1993 | JP |
05-235047 | Sep 1993 | JP |
05-251339 | Sep 1993 | JP |
05-270997 | Oct 1993 | JP |
05-283336 | Oct 1993 | JP |
05-291152 | Nov 1993 | JP |
05-304334 | Nov 1993 | JP |
05-343327 | Dec 1993 | JP |
05-343685 | Dec 1993 | JP |
06-045606 | Feb 1994 | JP |
06-132236 | May 1994 | JP |
06-177381 | Jun 1994 | JP |
06-196809 | Jul 1994 | JP |
06-222388 | Aug 1994 | JP |
06-224138 | Aug 1994 | JP |
06-230421 | Aug 1994 | JP |
06-252057 | Sep 1994 | JP |
06-291048 | Oct 1994 | JP |
07-070752 | Mar 1995 | JP |
07-086269 | Mar 1995 | JP |
07-300649 | Nov 1995 | JP |
08-181076 | Jul 1996 | JP |
08-245291 | Sep 1996 | JP |
08-264530 | Oct 1996 | JP |
09-260786 | Oct 1997 | JP |
09-293681 | Nov 1997 | JP |
10-188840 | Jul 1998 | JP |
10-190128 | Jul 1998 | JP |
10-308283 | Nov 1998 | JP |
11-269652 | Oct 1999 | JP |
2000-031387 | Jan 2000 | JP |
2000-058777 | Feb 2000 | JP |
2000-068072 | Mar 2000 | JP |
2000-087029 | Mar 2000 | JP |
2000-138094 | May 2000 | JP |
2000-178735 | Jun 2000 | JP |
2000-218445 | Aug 2000 | JP |
2000-319772 | Nov 2000 | JP |
2000-340883 | Dec 2000 | JP |
2000-353666 | Dec 2000 | JP |
2001-020075 | Jan 2001 | JP |
2001-62244 | Mar 2001 | JP |
2001-152339 | Jun 2001 | JP |
2001-172767 | Jun 2001 | JP |
2001-189312 | Jul 2001 | JP |
2001-217206 | Aug 2001 | JP |
2001-220287 | Aug 2001 | JP |
2001-220294 | Aug 2001 | JP |
2001-240972 | Sep 2001 | JP |
2001-254181 | Sep 2001 | JP |
2001-284042 | Oct 2001 | JP |
2001-303251 | Oct 2001 | JP |
2001-328900 | Nov 2001 | JP |
2002-60944 | Feb 2002 | JP |
2002-167672 | Jun 2002 | JP |
2002-172767 | Jun 2002 | JP |
2001-111000 | Dec 2002 | JP |
WO 9002216 | Mar 1990 | WO |
WO 9110510 | Jul 1991 | WO |
WO 9302111 | Feb 1993 | WO |
WO 9617107 | Jun 1996 | WO |
WO 9618756 | Jun 1996 | WO |
WO 9806889 | Feb 1998 | WO |
WO 9851838 | Nov 1998 | WO |
WO 9901595 | Jan 1999 | WO |
WO 9913504 | Mar 1999 | WO |
WO 9929924 | Jun 1999 | WO |
WO 9941423 | Aug 1999 | WO |
WO 0011721 | Mar 2000 | WO |
WO 0015865 | Mar 2000 | WO |
WO 0015881 | Mar 2000 | WO |
WO 0016377 | Mar 2000 | WO |
WO 0054320 | Sep 2000 | WO |
WO 0063957 | Oct 2000 | WO |
WO 0079019 | Dec 2000 | WO |
WO 0079576 | Dec 2000 | WO |
WO 0115220 | Mar 2001 | WO |
WO 0127346 | Apr 2001 | WO |
WO 0127347 | Apr 2001 | WO |
WO 0129280 | Apr 2001 | WO |
WO 0129891 | Apr 2001 | WO |
WO 0129893 | Apr 2001 | WO |
WO 0136702 | May 2001 | WO |
WO 0140541 | Jun 2001 | WO |
WO 0166832 | Sep 2001 | WO |
WO 0201628 | Jan 2002 | WO |
WO 0245167 | Jun 2002 | WO |
WO 0245871 | Jun 2002 | WO |
WO 0246489 | Jun 2002 | WO |
WO 0267319 | Aug 2002 | WO |
Number | Date | Country | |
---|---|---|---|
20060009034 A1 | Jan 2006 | US |
Number | Date | Country | |
---|---|---|---|
11038592 | Jan 2005 | US | |
11038592 | Jan 2005 | US | |
60305765 | Jul 2001 | US |
Number | Date | Country | |
---|---|---|---|
Parent | 10268195 | Oct 2002 | US |
Child | 10879448 | US | |
Parent | 09678266 | Oct 2000 | US |
Child | 10762764 | US |
Number | Date | Country | |
---|---|---|---|
Parent | 10418728 | Apr 2003 | US |
Child | 11038592 | US | |
Parent | 10268195 | Oct 2002 | US |
Child | 10418728 | US | |
Parent | 10879448 | Jun 2004 | US |
Child | 10268195 | US | |
Parent | 10762764 | Jan 2004 | US |
Child | 10268195 | US | |
Parent | 09605593 | Jun 2000 | US |
Child | 09678266 | US | |
Parent | 10196514 | Jul 2002 | US |
Child | 09605593 | US |