The present disclosure relates to atomic-layer deposition (ALD), and in particular relates to oxygen radical enhanced ALD, wherein an ozone plasma is used to generate the oxygen radicals.
The entire disclosure of any publication or patent document mentioned herein is incorporated by reference.
Atomic layer deposition (ALD) is a method of depositing a thin film on a substrate in very controlled manner. The deposition process is controlled by using two or more chemicals (“precursors”) in vapor form and reacting them sequentially and in a self-limiting manner on the substrate surface. The sequential process is repeated to build up the thin film layer by layer, wherein the layers are atomic scale.
ALD is used to form a wide variety of films, such as binary, ternary and quaternary oxides for advanced gate and capacitor dielectrics, as well as metal-based compounds for interconnect barriers and capacitor electrodes. An overview of the ALD process is presented in the article by George, entitled “Atomic Layer Deposition: an Overview,” Chem. Rev. 2010, 110, pp 111-113 (published on the Web on Nov. 20, 2009).
One type of ALD is called radical enhanced ALD (RE-ALD). RE-ALD utilizes radicals generated by a plasma to form one of the precursor gases. Because a radicalized precursor tends to be more reactive than its unradicalized counterpart, it helps induce the reactions when forming the film layers.
The type of plasma used in RE-ALD is referred to by the name of the feedgas used to form the plasma. For example, an “oxygen plasma” utilizes oxygen (O2) as the feedgas to produce a plasma that generates oxygen-radicals precursors. The oxygen-radical precursors comprise monatomic oxygen, which has two unpaired electrons that make monatomic oxygen very reactive. The oxygen radicals serve as co-reactants that are used in conjunction with a second precursor (say, Si). The two precursors are feed sequentially into the reactor chamber to produce sequential layers that lead to thin film growth (e.g., SiO2).
While ALD has many advantages, one of its major disadvantages as compared to other film growth processes (such as chemical-vapor deposition or CVD) is that it is quite slow. For example, a conventional ALD reactor has a growth rates measured in angstroms/minute, while CVD has growth rates measured in microns/minute. Slow growth rates result in excellent film quality but limit the throughput of processed substrates (wafers) in a semiconductor manufacturing line. Thus, while an oxygen plasma is effective in providing oxygen-radical precursors for oxygen-based RE-ALD, there is always a need to increase the speed and/or efficiency of an oxygen-based RE-ALD process.
An aspect of the disclosure is a method of performing a radical enhanced atomic-layer deposition (RE-ALD) process on a surface of a substrate that resides within an interior of a reactor chamber. The method includes: forming an ozone plasma to generate oxygen radicals (O*); and sequentially feeding the oxygen radicals and a precursor gas into the interior of the reactor chamber to form an oxide film on the substrate surface.
Another aspect of the disclosure is the method described above, wherein the ozone plasma is inductively formed within a plasma tube that is operably (e.g., pneumatically) coupled to the interior of the reactor chamber.
Another aspect of the disclosure is the method described above, wherein the precursor gas comprises a metal organic precursor.
Another aspect of the disclosure is the method described above, wherein the metal organic precursor is selected from the group comprising: silicon, aluminum, hafnium, titanium, zirconium, tantalum, yttrium and magnesium.
Another aspect of the disclosure is the method described above, wherein the oxide film comprises a metal oxide.
Another aspect of the disclosure is the method described above, wherein the metal oxide is selected from the group comprising: SiO2, Al2O3, HfO2, TiO2, ZrO2, Ta2O5, Y2O3 and Mg2O4.
Another aspect of the disclosure is the method described above, including introducing a purge gas into the interior of the reactor chamber to assist in purging the interior of the reactor chamber.
Another aspect of the disclosure is the method described above, wherein the generating of the oxygen radicals O* includes dissociating an ozone molecule to form diatomic oxygen molecule O2 and a first oxygen radical O*, and then dissociating the diatomic oxygen molecule O2 to form second and third oxygen radicals O*.
Another aspect of the disclosure is the method described above, wherein the substrate comprises a silicon wafer.
Another aspect of the disclosure is a method of performing a RE-ALD process on a surface of a substrate that resides within an interior of a reactor chamber. The method includes: providing a first precursor gas comprising oxygen radicals O* by forming an ozone plasma from ozone gas within a plasma tube, wherein the plasma tube is pneumatically coupled to the interior of the reactor chamber; providing a second precursor gas from a gas source that is pneumatically coupled to the interior of the reactor chamber; and sequentially introducing the first precursor gas and the second precursor gas into the interior of the reactor chamber to form an oxide film on the substrate surface.
Another aspect of the disclosure is the method described above, wherein one of the first and second precursor gases comprises at least one of: silicon, aluminum, hafnium, titanium, zirconium, tantalum, yttrium and magnesium.
Another aspect of the disclosure is the method described above, wherein the oxide film comprises one of: SiO2, Al2O3, HfO2, TiO2, ZrO2, Ta2O5, Y2O3 and Mg2O4.
Another aspect of the disclosure is the method described above, including introducing a purge gas into the interior of the reactor chamber to assist in purging the interior of the reactor chamber.
Another aspect of the disclosure is the method described above, wherein the substrate comprises a silicon wafer.
Another aspect of the disclosure is the method described above, wherein the plasma tube is made of quartz.
Another aspect of the disclosure is the method described above, wherein forming the ozone plasma includes subjecting the ozone in the plasma tube to inductive coupling.
Another aspect of the disclosure is the method described above, wherein forming the oxygen radicals O* includes: dissociating an ozone molecule to form diatomic oxygen molecule O2 and a first oxygen radical O*; and dissociating the diatomic oxygen molecule O2 to form second and third oxygen radicals O*.
Another aspect of the disclosure is a system for performing a RE-ALD process on a surface of a substrate. The system includes: a reactor chamber having an interior configured to support the substrate; an ozone plasma system pneumatically connected to the interior of the reactor chamber and configured to form an ozone plasma that generates oxygen radicals O*; a gas source pneumatically coupled to the interior of the reactor chamber and that contains a gas; a vacuum pump pneumatically connected to the interior of the reactor chamber; and a controller operably connected to the ozone plasma system, the vacuum pump and the gas source. The controller is configured to introduce the oxygen radicals and the gas sequentially into the interior of the reactor chamber to form an oxide film on the substrate surface.
Another aspect of the disclosure is the system described above, wherein the ozone plasma system forms the oxygen radicals O* by dissociating an ozone molecule to form diatomic oxygen molecule O2 and a first oxygen radical O*, and then dissociating the diatomic oxygen molecule O2 to form second and third oxygen radicals O*.
Another aspect of the disclosure is the system described above, wherein the gas includes one of: silicon, aluminum, hafnium, titanium, zirconium, tantalum, yttrium and magnesium.
Another aspect of the disclosure is the system described above, wherein the plasma system includes an inductively coupled plasma source.
Another aspect of the disclosure is the system described above, further comprising the substrate, wherein the substrate comprises silicon.
Additional features and advantages are set forth in the Detailed Description that follows, and in part will be readily apparent to those skilled in the art from the description or recognized by practicing the embodiments as described in the written description and claims hereof, as well as the appended drawings. It is to be understood that both the foregoing general description and the following Detailed Description are merely exemplary, and are intended to provide an overview or framework to understand the nature and character of the claims.
The accompanying drawings are included to provide a further understanding, and are incorporated in and constitute a part of this specification. The drawings illustrate one or more embodiment(s), and together with the Detailed Description serve to explain principles and operation of the various embodiments. As such, the disclosure will become more fully understood from the following Detailed Description, taken in conjunction with the accompanying Figures, in which:
Reference is now made in detail to various embodiments of the disclosure, examples of which are illustrated in the accompanying drawings. Whenever possible, the same or like reference numbers and symbols are used throughout the drawings to refer to the same or like parts. The drawings are not necessarily to scale, and one skilled in the art will recognize where the drawings have been simplified to illustrate the key aspects of the disclosure.
The claims as set forth below are incorporated into and constitute part of this Detailed Description.
In the discussion herein, an oxygen radical is denoted as O* and represents monatomic oxygen, which has a total of six electrons, two of which are unpaired. The unpaired electrons make O* very reactive, i.e., more reactive than ozone (O3), which is more reactive than diatomic oxygen (O2).
In the discussion below, oxygen radicals O* constitute a first precursor gas that serves as an oxidizing precursor, while a second precursor gas is a non-oxide gas that forms, in combination with the first precursor gas, a thin-film oxide compound on a substrate surface.
RE-ALD system 10 also includes precursor gas source 50 that is pneumatically connected to reactor chamber interior 26 and that provides a precursor gas 52 to the reactor chamber interior as part of the RE-ALD process. In an example, precursor gas 52 is any gas that combines with oxygen to form oxide layer 142 on wafer surface 42. Example first precursor gases include: silicon (e.g., to form SiO2), aluminum (e.g., to form Al2O3), hafnium (e.g., to form HfO2), titanium (e.g., to form TiO2), zirconium (e.g., to form ZrO2), tantalum (to form Ta2O5), Yttrium (e.g., to form Y2O3) and magnesium (e.g., to form Mg2O4).
RE-ALD system 10 further includes an optional second gas source 60 that is pneumatically connected to reactor chamber interior 26 and that provides an inert gas 62 to the reactor chamber interior. Inert gas 62 serves as a purge gas between introducing the different precursor gasses to speed up the sequential layering processes when forming oxide film 142. Note that the second gas source 60 can be combined with precursor gas source 50 so that the precursor gas 52 and the inert gas 62 can flow into reactor chamber interior 26 through the same conduit.
RE-ALD system 10 also includes an ozone plasma system 100 that is pneumatically coupled to reactor chamber interior 26.
An example ozone plasma system 100 includes an ozone gas source 110 that contains ozone gas 112. The ozone gas source 110 is pneumatically coupled to an input end 122 of a plasma tube 120. Plasma tube 20 also has output end 123, an outer surface 124 and an interior 126. An example plasma tube 120 is made of quartz and is substantially cylindrical. A radio-frequency (RF) coil 130 resides around outer surface 124 of plasma tube 120 and is operably connected to an RF source 134. The RE-ALD system 10 can include a number of valves 150 that are used to control the flow of precursor gas 52, inert purge gas 62, ozone gas 112, as well as the pneumatic connection of vacuum pump 46, to reactor chamber interior 26. The valve 150 at the output end of ozone gas source 100 adjacent reactor chamber 20 is optional and may not be required given the low pressure in reactor chamber interior 26.
The RE-ALD system 10 also includes a controller 200 operably connected to ozone plasma system 100 and valves 150. Controller 200 is configured to control the operation of the RE-ALD system to form oxide film 142 on substrate surface 42. In particular, controller 200 is configured to control the opening and closing of valves 150 as needed to perform the sequential introduction of precursor gases 116 and 52 into chamber interior 16, including the removal of one precursor gas before introducing the other precursor gas. In an example, controller 200 controls the introduction of purge gas 62 to assist in removing one of the precursor gases 116 or 52 from reactor chamber interior 26 prior to introducing the other precursor gas into the reactor chamber interior.
With reference to
Thus, a single ozone atom in ozone gas 112 ends up forming three oxygen radicals O* (i.e., 3O*) that enter reactor chamber interior 26 as oxidizing precursor gas 116. This is in contrast to prior-art RE-ALD systems that utilize an oxygen plasma, wherein diatomic oxygen O2 is the feedgas. A single diatomic oxygen molecule O2 will only be able to generate two oxygen radicals O*. Thus, ozone plasma 114 can produce ⅓ more monatomic oxygen radicals O* than an oxygen plasma. The increased oxygen radical density increases the growth rate of oxide film 142.
Furthermore, since ozone O3 is more reactive than diatomic oxygen O2, the amount of energy it takes to generate the oxygen radicals O* is less on average for ozone plasma 114 than for an oxygen plasma. That is, the formation of oxygen radicals O* by the dissociative reaction O3+e−→O2+O* takes less energy than the formation of the oxygen radicals formed by the dissociative reaction O2+e−2O*. Also, the reaction O3+e−→O2+O* occurs at a rate of 1.9×10−9 cm3/s while the reaction O2+e−→2O* occurs at a rate of 8.6×10−10 cm3/s. The complete dissociation of ozone into three oxygen radicals O* produces oxygen radicals at greater than twice the rate when dissociating oxygen only.
Thus, with continuing reference to
It will be apparent to those skilled in the art that various modifications to the preferred embodiments of the disclosure as described herein can be made without departing from the spirit or scope of the disclosure as defined in the appended claims. Thus, the disclosure covers the modifications and variations provided they come within the scope of the appended claims and the equivalents thereto.
This application claims priority under 35 U.S.C. §119(e) of U.S. Provisional Patent Application Ser. No. 61/970,820, filed on Mar. 26, 2014, and which is incorporated herein by reference.
Number | Name | Date | Kind |
---|---|---|---|
6933011 | Senzaki | Aug 2005 | B2 |
7128787 | Castovillo et al. | Oct 2006 | B2 |
7205247 | Lee et al. | Apr 2007 | B2 |
7407876 | Ishizaka | Aug 2008 | B2 |
8163087 | Faguet et al. | Apr 2012 | B2 |
8168375 | Nakajima et al. | May 2012 | B2 |
8336490 | Matsuura et al. | Dec 2012 | B2 |
8486845 | Matsuda | Jul 2013 | B2 |
20030140671 | Lande | Jul 2003 | A1 |
20040020601 | Zhao | Feb 2004 | A1 |
20050239297 | Senzaki et al. | Oct 2005 | A1 |
20060051505 | Kortshagen | Mar 2006 | A1 |
20060054184 | Mozetic | Mar 2006 | A1 |
20060063346 | Lee | Mar 2006 | A1 |
20060276018 | Nam | Dec 2006 | A1 |
20090056877 | Matsuura et al. | Mar 2009 | A1 |
20100075067 | Kim | Mar 2010 | A1 |
20110143053 | Shirahata | Jun 2011 | A1 |
20110151619 | Orita | Jun 2011 | A1 |
20110183079 | Jackson et al. | Jul 2011 | A1 |
20120021590 | Ishii | Jan 2012 | A1 |
20120255612 | Pierreux | Oct 2012 | A1 |
20130012033 | Kabe et al. | Jan 2013 | A1 |
20130125815 | Liu et al. | May 2013 | A1 |
20130216708 | Yun | Aug 2013 | A1 |
20130295779 | Chandra et al. | Nov 2013 | A1 |
20130313657 | Tong | Nov 2013 | A1 |
Number | Date | Country |
---|---|---|
2481830 | Aug 2012 | EP |
Entry |
---|
Niskanen, Antti, et al., “Radical Enhanced Atomic Layer Deposition of Tantalum Oxide”. Chem. Mater. 2007, 19, 2316-2320. |
Edy, Riyanto, et al., “Influence of argon plasma on the deposition of Al2O3 film onto the PET surfaces by atomic layer deposition”. Nanoscale Research Letters, 2013, 8:79, pp. 1-9. |
Sundstrom, Hans, et al., “Ozone as the Oxidizing Precursor in Atomic Layer Deposition”. Gas & Chemicals, Dec. 2005, www.eurosemi.eu.com, G1-G3. |
Niskanen, Antti, et al., “Radical Enhanced Atomic Layer Deposition of Titanium Dioxide”. Chemical Vapor Deposition, 2007, 13, 152-157. |
George, “Atomic Layer Deposition: An Overview,” Chem. Rev. 2010, 110, pp. 111-131 (published on the web on Nov. 20, 2009). |
Niskanen, “Radical enhanced atomic layer deposition of metals and oxides,” Academic Dissertation, University of Helsinki, Nov. 10, 2006. |
Sundstrom, “Ozone as the oxidizing precursor in atomic layer deposition,” Gas & Chemicals G1, www.eurosemi.eu.com Dec. 2005. |
Vandenbroucke, “Modeling and experimental validation of TCE abatement and ozone formation with non thermal plasma,” 8th International Symposium on Non-Thermal/Thermal Plasma Pollution Control Technology and Sustainable Energy, Proceedings, 2012. |
Werner, “High-rate atomic layer deposition of Al2O3 for the surface passivation of Si solar cells,” Energy Procedia 8 (2011) pp. 301-306. |
Office Action from Japanese Patent office dated Feb. 26, 2016, for Japanese counterpart Patent Application No. 2015-022812. |
Number | Date | Country | |
---|---|---|---|
20150279665 A1 | Oct 2015 | US |
Number | Date | Country | |
---|---|---|---|
61970820 | Mar 2014 | US |