Embodiments of the present disclosure generally relate to deposition of materials. Another field of the present disclosure is semi-conductor device fabrication technology. Particular applications of the present disclosure include the formation of silicon layers.
A sub 400° C. ALD process for growing monolayers of Si on clean surfaces by alternating pulses of Si2H6 and SiCl4 employed with the substrate temperature varied between 355°-385° C. The process is slow, with each ALD cycle taking several minutes and the desorption of the HCl(g) byproduct being slow below 400° C. Other processes include monolayer silicon ALD growth on Ge with use of alternating pulses of Si2Cl6 and atomic hydrogen, or Si2Cl6 and Si2H6, at undesirably high substrate temperatures of 400°-465° C.
Physical vapor deposition (PVD) of silicon for passivation of III-V surfaces has been reported, but requires a silicon multilayer as the silicon is not ordered. Also, the PVD deposition of silicon is not compatible with processing of three dimensional devices such as finFETs on large semiconductor wafers.
In one embodiment, a method for depositing silicon on a semiconductor or metallic surface comprises cycling dosing of silane and chlorosilane precursors at a temperature between 50° C. and 300° C. and continuing cycling between three and twenty three cycles until the deposition self-limits via termination of surface sites with Si—H groups.
In another embodiment, a method of layer formation comprises depositing a chlorosilane onto a substrate to form a first layer, wherein the substrate is selected from the group consisting of InxGa1-xAs, InxGa1-xSb, InxGa1-xN, SiGe, and Ge, wherein X is between 0.1 and 0.99. The method may include pulsing a silane to form a silicon monolayer. The method may include cycling dosing of the chlorosilane and the silane.
In another embodiment, a layered composition comprises a first layer selected from the group consisting of InxGa1-xAs, InxGa1-xSb, InxGa1-xN, SiGe, and Ge, wherein X is between 0.1 and 0.99, and a second layer, wherein the second layer comprises Si—H and Si—OH.
In one embodiment, a method for depositing silicon on a semiconductor or metallic surface comprises cycling dosing of silane and chlorosilane precursors at a temperature between 50° C. and 300° C. and continuing cycling between three and twenty three cycles until the deposition self-limits via termination of surface sites with Si—H groups.
In another embodiment, a method of layer formation comprises depositing a chlorosilane onto a substrate to form a first layer, wherein the substrate is selected from the group consisting of InxGa1-xAs, InxGa1-xSb, InxGa1-xN, SiGe, and Ge, wherein X is between 0.1 and 0.99. The method may include pulsing a silane to form a silicon monolayer. The method may include cycling dosing of the chlorosilane and the silane.
In another embodiment, a layered composition comprises a first layer selected from the group consisting of InxGa1-xAs, InxGa1-xSb, InxGa1-xN, SiGe, and Ge, wherein X is between 0.1 and 0.99, and a second layer, wherein the second layer comprises Si—H and Si—OH.
Embodiments of the present disclosure may provide self-limiting and saturating atomic layer deposition (ALD) and self-limiting and saturating chemical vapor deposition (CVD) of a silicon seed layer on a variety of non-silicon layer surfaces. Embodiments of the present disclosure may include depositing a silicon seed layer on substrates of varying alloy compositions (e.g. indium gallium arsenide, indium gallium antiminide, indium gallium nitride, and silicon-germanium), as well as germanium and metallic substrates.
Embodiments of the present disclosure provide low temperature silicon ALD and can use different substrates. Embodiments provide a comparable drop in substrate temperature to 250° C. or less in addition to providing self-limiting and saturating ALD growth.
Artisans have failed, to the knowledge of the present inventors, to provide self-limiting and saturating silicon CVD on non-silicon surfaces despite studies and reports in the literature of temperature ranges at which hydrogen desorption occurs from similar applicable substrates of Si, Ge, and GaAs. The silane precursor self-limiting CVD process produces saturation when all surface sites are terminated by Si—H groups. Thus, desorption of H2(g) from substrate surface sites may occur until all surface sites become terminated by Si—H. Increase of substrate temperature to 400° C. leads to continued ALD silicon growth on top of the self-limiting ALD silicon seed layer or on top of the saturated self-limited CVD silicon seed layer.
For oxide deposition, metal contact deposition, surface functionalization, surface passivation, and oxide nucleation, methods of the present disclosure provide advantages compared to typical current semiconductor and metal substrate surface preparation and controlled growth methods.
Methods of the present disclosure may provide for improved semiconductor and metal substrate surface preparation and controlled growth methods. Functionalization creates a surface that is reactive to ALD precursors. Passivation forms a monolayer that leaves the Fermi level unpinned. The monolayer nucleation is the initial layer of ALD deposition. The process is low temperature. In one embodiment, preparation, functionalization, passivation and ALD deposition is performed at 250° C. Certain surfaces and substrates will permit lower temperatures. Substrates that recombinatively desorb H2 at lower temperatures, e.g., 150° C., permit use of lower temperatures. Examples include InGaAs and InAs.
Present silicon saturating and self-limiting ALD and CVD processes of the present disclosure achieve functionalization, passivation and monolayer nucleation at 250° C. (and lower for some substrates), which is much lower temperature, on both metallic and semiconductor substrates, than comparable silicon ALD procedures reported in literature. The self-limiting and saturating silicon CVD process at 250° C. is advantageous from a device fabrication standpoint compared to existing silicon ALD processes that are at significantly higher temperature (above 350° C.) and provide for continuous growth of silicon on silicon and is not self-limiting. A unique strong bonding of silicon to all crystal faces of InxGa1-xAs, InxGa1-xSb, InxGa1-xN, SiGe, and Ge should enable transfer of the dangling bonds from the substrate to silicon, and silicon is readily hydrogen passivated even by molecular H2 due to the uniquely strong Si—H bonds. The monolayer of —OH may be ideal for nucleating almost any metal ALD precursor.
The ability to passivate metallic surfaces provides additional applications beyond semiconductor device fabrication. For example, methods of the present disclosure can provide a surface protection against oxidation on metallic surfaces.
The present disclosure provides, for example, self-limiting and saturating atomic layer deposition (ALD) and self-limiting and saturating chemical vapor deposition (CVD) of a silicon seed layer on indium gallium arsenide (InGaAs), indium gallium antiminide (InGaSb), indium gallium nitride (InGaN), and silicon-germanium (SiGe) substrates of varying alloy compositions, as well as germanium and metallic substrates. Embodiments of the present disclosure also provide a procedure for ALD silicon on top of the self-limiting ALD silicon seed layer or on top of the saturated self-limited CVD silicon seed layer for continued growth of silicon.
A silicon monolayer deposited as described herein can serve several purposes. (1) The dangling bonds of the substrate will be transferred to silicon, which are then passivated by hydrogen, leaving the surface electrically passivated. (2) The saturated monolayer of silicon with H passivation will serve to protect the semiconductor or metallic substrate from oxidation. (3) The silicon monolayer with possible H termination (e.g. Si—H) can also be employed for deposition of gate oxide through functionalization by an oxidant such as HOOH(g), in order to create an Si—OH layer which would react with nearly any ALD precursor thereby eliminating the need for metal precursor nucleation (for example with trimethyl aluminum predosing) decreasing EOT and lowering border trap density and fixed charge associated with interfacial layers or even direct bonding of oxide to nonsilicon semiconductors. The same procedure can be used for other crystallographic faces such as InxGa1-xAs(110), InxGa1-xSb(110), InxGa1-xN(110), SiGe(110), and Ge(110). Some ALD precursors such as those containing O or OH groups may directly react with the Si—H termination. (4) The silicon monolayer or silicon monolayer with additional oxide ALD can be employed for metal contact formation.
Experiments of the present disclosure will be understood by artisans in view of the general knowledge in the art and the description that follows to illustrate broader features of some embodiments of the present disclosure.
The experiments showed self-limiting ALD of silicon on semiconductor and metal surface. Dosing parameters for near saturation coverage of silicon on clean InGaAs surface through cyclic dosing of Si2Cl6 and Si3H8 were shown. Scanning Tunneling Microscopy (STM) and X-Ray Photoelectron Spectroscopy (XPS) measurements were performed to investigate surface bonding configurations and electronic structures of Si/InGaAs(001)-(2×4). Thermal annealing measurements were also performed during this time to demonstrate thermal stability of the surface.
The experiments also show self-limiting CVD of silicon on semiconductor and metal surfaces through dosing of Si3Ha. Dosing parameters were determined for near saturation coverage of silicon on clean InGaAs surface. STM and XPS measurements were used to investigate surface bonding configurations and electronic structures of silicon/InGaAs(001)-(2×4). Thermal annealing measurements were also performed during this time to demonstrate thermal stability of the surface.
One embodiment includes a self-limiting atomic layer deposition procedure based upon the saturation of the substrate semiconductor or metallic surface sites through a surface termination with Si—H and Si—Cl groups by cyclic dosing of silane and chlorosilane precursors at 250° C. Silane precursors include: SiH4, Si2H6, Si3H8, Si4H10, Si5H12 and chlorosilane precursors include: SiCl4, Si2Cl6, Si3Cl8. Once all surface sites are terminated with Si—H and Si—Cl groups, the reaction becomes self-terminating, as hydrogen and chlorine bond to silicon stronger than other semiconductor or metallic materials. The self-limiting and saturating chemical vapor deposition procedure is based upon the saturation of the substrate semiconductor or metallic surface sites through a surface termination with Si—H groups by dosing a silane precursor at 250° C. Once surface sites are terminated with Si—H groups, the reaction becomes self-terminating, as hydrogen bonds to silicon stronger than other semiconductor or metallic materials. Further silicon growth can occur on either the self-limiting atomic layer deposition or chemical vapor deposition saturated surfaces by raising the temperature to 400° C. The H2(g) and HCl(g) desorption product occurs only slowly below this temperature at the point of surface saturation.
The self-limiting atomic layer deposition procedure in an experiment is discussed next. A decapped In0.53Ga0.47As(001)-(2×4) surface was dosed with 1 MegaLangmuir of Si2Cl6 followed by 1 MegaLangmuir of Si3H8 at a sample temperature of 250° C. This procedure constitutes one complete self-limiting and saturating ALD cycle. After three cycles, an X-ray photoelectron spectroscopy (XPS) spectrum is taken of the surface with a non-monochromatic aluminum channel X-ray flood source system at a glancing angle of 30° to produce surface sensitive spectra. The XPS spectra were also recorded following 13 and 23 total self-limiting and saturating ALD cycles.
As shown in
The raw counts corrected by Schofield photoionization cross sectional relative sensitivity factors are recorded for doublet peak pairs of As 2p, Ga 2p, In 3d, Si 2p, Cl 2p for the clean decapped In0.53Ga0.47As(001)-(2×4) surface (100) as well as the 3, 13, and 23 ALD cycle dosed surfaces at sample temperature 250° C. (102, 104 and 106, respectively) and are shown in Table 1.
The raw counts corrected by Schofield photoionization cross sectional relative sensitivity factors are recorded and listed in Table 2 as relative atomic ratios compared to the total As 3d peak. All peaks ratios tabulated in Table 2 are from comparable low binding energies, including: Ga 3d, In 3d, Si 2p, Cl 2p, and Ta 4d total peak values for both doublet peak pairs, as well as the O 1s, C 1s peaks. Ratios are listed for the clean decapped In0.53Ga0.47As(001)-(2×4) surface (100) as well as the 3, 13, and 23 ALD cycle dosed surfaces at sample temperature 250° C. (102, 104 and 106, respectively). As shown in Table 2 and
The filled-state STM image may be obtained of In0.53Ga0.47As(001)-(2×4) surface following 23 self-limiting and saturating ALD cycles of 1 MegaLangmuir of Si2Cl6 followed by 1 MegaLangmuir of Si3H8 at a sample temperature of 250° C. as compared to the clean decapped In0.53Ga0.47As(001)-(2×4) surface. The dosed surface contains high atomic surface order and the surface should be terminated by Si—H, leaving the surface Fermi level unpinned.
The self-limiting and saturating CVD procedure may include a decapped In0.53Ga0.47As(001)-(2×4) surface dosed with 1 MegaLangmuir of Si3H8 at a sample temperature of 250° C. This procedure constitutes one complete self-limiting and saturating CVD cycle. After three cycles, an X-ray photoelectron spectroscopy (XPS) spectrum is taken of the surface with a non-monochromatic aluminum channel X-ray flood source system at a glancing angle of 30° to produce surface sensitive spectra. The XPS spectra were also recorded following 13 total self-limiting and saturating CVD cycles.
As shown in
The raw counts corrected by Schofield photoionization cross sectional relative sensitivity factors are recorded for doublet peak pairs of As 2p, Ga 2p, In 3d, Si 2p, Cl 2p for the clean decapped In0.53Ga0.47As(001)-(2×4) surface (200) as well as the 3 and 13 CVD cycle dosed surfaces at sample temperature 250° C. (202 and 204, respectively) and are shown in Table 3. The Ga 3p3/2 peak continues to diminish with 13 cycles (204) and near saturation of silicon on In0.53Ga0.47As(001)-(2×4) surface is reached after 13 self-limiting and saturating CVD cycles at 250° C. (204). H2 desorption is close to zero at 250° C. on silicon.
The self-limiting and saturating CVD procedure includes a decapped In0.53Ga0.47As(001)-(2×4) surface dosed with 1 MegaLangmuir of Si3H8 at a sample temperature of 250° C. This procedure constitutes one complete self-limiting and saturating CVD cycle. After three cycles, an XPS spectrum is taken of the surface with a non-monochromatic aluminum channel X-ray flood source system at a glancing angle of 30° to produce surface sensitive spectra. The XPS spectra were also recorded following 13 total self-limiting and saturating CVD cycles.
The raw counts corrected by Schofield photoionization cross sectional relative sensitivity factors are recorded and listed in Table 4 as relative atomic ratios compared to the total As 3d peak. All peaks ratios tabulated in Table 4 are from comparable low binding energies, including: Ga 3d, In 3d, Si 2p, Cl 2p, and Ta 4d total peak values for both doublet peak pairs, as well as the O 1s, C 1s peaks. Ratios are listed for the clean decapped In0.53Ga0.47As(001)-(2×4) surface (200) as well as for the 3 and 13 self-limiting and saturating CVD cycle dosed surfaces at sample temperature 250° C. (202 and 204, respectively). As shown in Table 4 and
Many applications will be apparent to artisans from the above discussion. Particular applications include that the CVD or ALD deposited silicon monolayer is applicable for use as a semiconductor and metallic surface protection layer from unwanted oxidation. This application may serve useful during deposition and processing of gate stacks on FinFETs for MOSFETs. Embodiments of the present disclosure may provide surface termination by Si—H groups followed by functionalization with an oxidant, creating an Si—OH layer, which can be performed prior to oxide gate deposition and source drain contact formation. The same process can be used for a monolayer oxide on unpinning of source/drain contacts on MOSFETs which is critical for SiGe. The same process can be used in flash memory where thin high-k oxides are needed for low voltage operation.
While specific embodiments of the present disclosure have been shown and described, it should be understood that other modifications, substitutions and alternatives are apparent to one of ordinary skill in the art. Such modifications, substitutions and alternatives can be made without departing from the spirit and scope of the present disclosure, which should be determined from the appended claims.
Various features of the present disclosure are set forth in the appended claims.
This application claims benefit of U.S. patent application Ser. No. 14/561,525, filed Dec. 5, 2014, which is herein incorporated by reference in its entirety, which claims priority to U.S. Provisional Patent Application Ser. No. 61/912,930, filed Dec. 6, 2013, which is herein incorporated by reference in its entirety.
Number | Name | Date | Kind |
---|---|---|---|
9305780 | Edmonds | Apr 2016 | B2 |
20110262642 | Xiao et al. | Oct 2011 | A1 |
Entry |
---|
B. Shin, et al., Pre-atomic Layer Deposition Surface Cleaning and Chemical Passivation of (100) in 0.2 Ga 0.8 as and Deposition of Ultrathin Al 2 O 3 Gate Insulators, Appl. Phys. Lett., 93, 052911 (2008). |
S. Yokoyama, et al., Self-Limiting Atomic-Layer Deposition of Si on SiO2 by Alternate Supply of Si2H6 and SiCl4, Appl. Phys. Lett., 79 (5), (2001). |
D. Koleske, et al., Atomic Layer Epitaxy of Si on Ge(100) Using Si2Cl6 and Atomic Hydrogen, Appl. Phys. Lett., 64(7), (1994). |
E. Hasunuma, et al., Gas-phase-reaction-controlled Atomic-layer-epitaxy of Silicon, J. Vac. Sci. Technol. A, 16(2), (1998). |
J. Lee, et al., Kinetics of H 2 ( D 2 ) Desorption from a Ge (100)−2×1: H (D) Surface Studied Using Scanning Tunneling Microscopy and Temperature Programmed Desorption, J. Chem. Phys., 118, 1929, (2003). |
P. Gupta, et al., Hydrogen Desoprtion Kinetics from Monohydride and Dihydride Species on Silicon Surfaces, Phys. Rev. B, 37, 8234, (1988). |
M. Akazawa, et al., High-k Al2O3 MOS Structures with Si Interface Control Layer Formed on Air-exposed GaAs and InGaAs Wafers, Appl. Surf. Sci., 256, 5708, (2010). |
M. El Kazzi, et al., Sub-nm Equivalent Oxide Thickness on Si-passivated GaAs Capacitors with Low Dit , Appl. Phys. Lett., 99, 052102, (2011). |
H. Hasegawa, et al., Control of GaAs and InGaAs Insulator-Semiconductor and Metal-Semiconductor Interfaces by Ultrathin Molecular Beam Epitaxy Si Layers, Jpn. J. Appl. Phys., 30, 3744, (1991). |
Office Action for U.S. Appl. No. 14/561,525 dated Aug. 31, 2015. |
Number | Date | Country | |
---|---|---|---|
20160190030 A1 | Jun 2016 | US |
Number | Date | Country | |
---|---|---|---|
61912930 | Dec 2013 | US |
Number | Date | Country | |
---|---|---|---|
Parent | 14561525 | Dec 2014 | US |
Child | 15060795 | US |