This disclosure relates to methods of processing workpieces and, more particularly, to altering the etch rate of materials disposed on workpieces using ion implantation.
Semiconductor fabrication comprises many discrete processes to create the desired features or devices. Some of these processes include lithography, etching, deposition and ion implantation.
Often, in the case of etching, a material, also referred to as a mask or hard mask, is disposed on the surface to be etched. Portions of the hard mask are removed, creating openings that expose some material or the underlying workpiece. The opening in the hard mask after this process is referred to as the critical dimension (CD). There is an inherent CD variation across several similar structures, both within a die and across the workpiece. CD variability impacts circuit performance and reduction of this variability is beneficial.
The exposed material or underlying workpiece is then treated with an etching process, which removes the exposed material or underlying workpiece.
This etching process functions due to the difference in etch rate between the hard mask and etch rate of the underlying material or workpiece. In other words, the etching process removes the material or underlying workpiece at a faster rate than it removes the hard mask. In this way, the exposed material or workpiece is etched, while the hard mask protects other portions of the workpiece.
However, as semiconductor fabrication processes continue to evolve, the initial openings in the hard mask prior to the etching process are becoming narrower. A narrower opening implies that either a longer or more aggressive etching process is performed to remove the desired amount of material or underlying workpiece.
This longer or more aggressive etching process may remove material from the hard mask and/or modify the hard mask shape. If too much of the hard mask is removed, the hard mask will no longer be able to protect the rest of the workpiece from the etching process. If the hard mask shape is modified during the etch process, the resulting CD may be different from the intended value. This effect creates an inherent CD variation across the die and workpiece. To compensate for this more aggressive etching process, the hard mask may be made thicker, to account for the removal of the hard mask by the etching process. In another embodiment, a different type of material, which is more resistant to etching, may be used for the hard mask.
However, these changes may cause modifications to the semiconductor fabrication process, which may be expensive or difficult to implement or may result in increased CD variation. Therefore, it would be advantageous if there was a method to modulate the etch resistance of the hard mask and other materials to allow currently used materials to continue to be exploited. Further, it would be beneficial if this method did not affect the overall throughput of the semiconductor fabrication process.
As etching processes become more aggressive, increased etch resistivity of the hard mask is desirable. Methods of modulating the etch rate of the mask and optionally the underlying material are disclosed. An etch rate modifying species is implanted into the hard mask after the mask etching process is completed. This etch rate modifying species increases the difference between the etch rate of the mask and the etch rate of the underlying material to help preserve the integrity of the mask during a subsequent etching process. In some embodiments, the etch rate of the mask is decreased by the etch rate modifying species. In certain embodiments, the etch rate of the underlying material is increased by the etch rate modifying species.
According to one embodiment, a method of processing a workpiece is disclosed. The method comprises creating an opening in a mask disposed on a surface of the workpiece, so as to expose a portion of a material disposed beneath the mask; implanting an etch rate modifying species into the mask and the portion of the material disposed beneath the mask; and etching the portion of the material disposed beneath the mask; wherein the etch rate modifying species increases a difference between an etch rate of the mask and an etch rate of the material. In certain embodiments, the etch rate modifying species decreases the etch rate of the mask. In certain embodiments, the etch rate modifying species increases the etch rate of the material. In certain embodiments, a layer is disposed between the workpiece and the mask, which may be a silicon dioxide layer. In certain embodiments, the material comprises the workpiece.
According to another embodiment, a method of processing a workpiece is disclosed. The method comprises creating an opening in a mask disposed on an epitaxial silicon layer, the epitaxial silicon layer disposed on a surface of the workpiece, so as to expose a portion of the epitaxial silicon layer disposed beneath the mask; implanting a first etch rate modifying species into the mask after creating the opening; and performing an etching process to create a channel in the portion of the epitaxial silicon layer, wherein the first etch rate modifying species decreases an etch rate of the mask. In certain embodiments, the first etch rate modifying species is implanted at an angle. In certain embodiments, the first etch rate modifying species comprises boron, carbon, silicon or germanium. In certain embodiments, the method further comprises implanting a second etch rate modifying species into the mask and the portion of the epitaxial silicon layer disposed beneath the mask prior to the etching process. In certain embodiments, the second etch rate modifying species increases the etch rate of the epitaxial silicon layer, and may comprise phosphorus, silicon, or antimony. In other embodiments, the second etch rate modifying species decreases the etch rate of the epitaxial silicon layer, and may comprise boron, carbon, aluminum, gallium or indium.
According to another embodiment, a method of processing a workpiece is disclosed. The method comprises creating an opening in a mask disposed on an silicon dioxide layer, the silicon dioxide layer disposed on a surface of the workpiece, so as to expose a portion of the silicon dioxide layer disposed beneath the mask; implanting an etch rate modifying species into the mask and the portion of the silicon dioxide layer; and etching the portion of the silicon dioxide layer; wherein the etch rate modifying species increases a difference between an etch rate of the mask and an etch rate of the silicon dioxide layer. In certain embodiments, the mask comprises silicon nitride. In certain embodiments, the etch rate modifying species is selected from the group consisting of boron and carbon.
For a better understanding of the present disclosure, reference is made to the accompanying drawings, which are incorporated herein by reference and in which:
The present disclosure describes the use of etching and ion implantation processes. Etching processes are well known in the art and may include either dry processes, such as via ion implantation, or wet processes, such as via the use of hydrofluoric acid or another acid. Similarly, ion implantation is well known in the art and may be achieved using a beam line ion implantation system, a plasma chamber, or any other suitable implantation system. The disclosure is not limited to any particular embodiment.
Vertical channels may be formed on the top surface of a workpiece. This may be done by applying a mask, such as a hard mask, to the entirety of the top surface of the workpiece. Openings are then created in the mask in those regions where the channels are intended to be disposed. The removal of the mask exposes the underlying material. In certain embodiments, the workpiece may be directly beneath the mask. In other embodiments, a layer, such as a silicon dioxide layer, may be disposed under the mask. The workpiece is then subjected to an etching process. The etching process attacks both the mask and the exposed material. However, since the mask is more resistant to the etching process, much more of the exposed material is etched, while the mask is able to protect the remainder of the workpiece.
Further, as noted above, as channels become narrower, the etching processes may be modified. For example, in certain embodiments, the etching process may be longer in terms of duration. In other embodiments, the etching process may be more aggressive, such as by increasing the energy used for an ion based etching process. These modifications may cause more of the mask to be removed or the shape of the mask to be altered. In certain embodiments, the entire mask may be etched by this modified etching process.
This may result in increased CD variability. A more etch resistant hard mask, which optionally may be made thinner, may reduce CD variability.
In one embodiment, this phenomenon is compensated for by modulating the etch rate of the mask, the underlying material, or both. Throughout this disclosure, the phrase “etch rate” is used to denote the rate at which material is removed by an etching process. The phrase “etch resistance” is used to denote a material's ability to withstand an etching process. Thus, an increase in etch resistance lowers the material's etch rate, while a decrease in etch resistance increases the material's etch rate.
The integrity of the mask during the etching process may be improved by increasing the etch rate of the underlying material as compared to the etch rate of the mask. This may be achieved in a number of ways. First, the etch resistance of the mask may be increased, while the etch resistance of the underlying material is not affected. Second, the etch resistance of the mask may be increased, while the etch resistance of the underlying material is decreased. Third, the etch resistance of the mask may be increased, while the etch resistance of the underlying material is also increased, but to a lesser degree. In each of these embodiments, the etch resistance of the mask is increased.
However, other embodiments are also possible. For example, the etch resistance of the underlying material may be lowered while the etch resistance of the mask is unaffected. In another embodiment, the etch resistance of the underlying material may be decreased, while the etch resistance of the mask is also decreased, but to a lesser degree.
In other words, in each of these embodiments, the integrity of the mask is improved by increasing the difference between the etch rate of the mask and the etch rate of the underlying material. The etch rate of the underlying material is always greater than the etch rate of the mask. However, by further increasing the difference between these two etch rates, less of the mask may be etched.
It has been discovered that this result can be achieved by the ion implantation of select species into the mask and the underlying material. These species may be referred to as etch rate modifying species.
In other embodiments, there may not be a layer 110. In such an embodiment, the mask 120 may be applied to the top surface of the workpiece 100, and the channel may be formed in the workpiece 100.
In
After the opening 125 has been created, an ion implantation process may be performed using an etch rate modifying species 140, as shown in
After the etch rate modifying species 140 has been implanted, the layer 110 is then etched to create channel 130, as shown in
In the embodiment where a layer 110 is not used, the etching process shown in
After the channel 130 has been created, subsequent processes may be performed, as shown in
Taking these results in combination, it can be demonstrated that if carbon is used as the etch rate modifying species 140 in
While boron and carbon show large decreases in the etch rate of the silicon nitride, other species may also be used. For example, an implant of nitrogen at a high current (HC) dose increases the etch rate of the silicon nitride by a factor of about 1.2, but increases the etch rate of the silicon dioxide layer by a factor of between 2.5 and 3.0. In other words, although the etch rate of the mask has been increased, the etch rate of the material being etched (i.e. layer 110) is increased to a greater degree.
While
Thus, in one particular embodiment, a silicon dioxide layer is disposed on the surface of a workpiece. A silicon nitride mask is then disposed on the silicon dioxide layer. Openings are made in the mask to allow for the creation of vertical channels in the silicon dioxide layer. After the openings are made, an ion implantation process using an etch rate modifying species is performed to change the etch rates of at least one of the mask and the silicon dioxide layer. The difference between the etch rate of the mask and the etch rate of the silicon dioxide layer is increased by the implantation of the etch rate modifying species. After the ion implantation is completed, an etching process is performed, to create the desired channel. In certain embodiments, the etch rate modifying species may be boron or carbon, due to their ability to decrease the etch rate of the silicon nitride mask.
In
After the opening 525 has been created, a first ion implantation process may be performed, as shown in
A second ion implantation process may be performed, as shown in
After the first and second ion implantation processes, an etching process is performed, as shown in
By implanting the first etch rate modifying species 540 and the second etch rate modifying species 550 prior to the etching process, the amount of mask 520 that is removed by the etching process may be reduced.
The implication of performing both ion implantation processes is that the silicon nitride hard mask thickness may be reduced. A thinner hard mask, coupled with a better etch resistance, will allow for reduced CD variability.
After the etching process has been completed, the channel 530 is created in the epitaxial silicon layer 510, as shown in
After the second ion implantation process, an etching process is performed to create the channel in the epitaxial silicon layer, as shown in Process 630. In certain embodiments, the introduction of the second etch rate modifying species may increase the etch rate of the epitaxial silicon layer. After the etching process is completed, a subsequent fabrication process, such as an ion implantation or metallization process, may be performed, as shown in Process 640.
The embodiments of this disclosure have many advantages. First, the use of an etch rate modifying species to modulate the etch rates of the mask and/or underlying material allows current processes and material to continue to be used in semiconductor fabrication. In other words, the currently used material for a mask may continue to be used, rather than transitioning to a new, more etch resistant material. Further, because of the increase in etch resistance, masks do not have to be made thicker to withstand the newer more aggressive etch processes and may optionally be made thinner. CD variability may be reduced by improving the hard mask etch resistance and optionally reducing the hard mask thickness. Further, the present disclosure offers methods to increase the resistance of hard masks without modification to their thickness or composition. The present disclosure also offers method to increase the etch rate of underlying silicon dioxide layers.
Further, these embodiments may be used in various applications, such as making nitride hard mask films more resistant to etch, increasing the etch rate of underlying silicon dioxide films in contact regions or decreasing the silicon dioxide etch rate in cases where silicon dioxide is being used as a hard mask, and increasing silicon etch rate during the formation of shallow trench isolation in FinFETs or decreasing silicon etch rate.
The present disclosure is not to be limited in scope by the specific embodiments described herein. Indeed, other various embodiments of and modifications to the present disclosure, in addition to those described herein, will be apparent to those of ordinary skill in the art from the foregoing description and accompanying drawings. Thus, such other embodiments and modifications are intended to fall within the scope of the present disclosure. Furthermore, although the present disclosure has been described herein in the context of a particular implementation in a particular environment for a particular purpose, those of ordinary skill in the art will recognize that its usefulness is not limited thereto and that the present disclosure may be beneficially implemented in any number of environments for any number of purposes. Accordingly, the claims set forth below should be construed in view of the full breadth and spirit of the present disclosure as described herein.
This application is a divisional application of U.S. patent application Ser. No. 14/975,968, filed Dec. 21, 2015, (now U.S. Pat. No. 9,934,982 issued Apr. 3, 2018), the disclosure of which is incorporated herein by reference in its entirety.
| Number | Name | Date | Kind |
|---|---|---|---|
| 5468342 | Nulty et al. | Nov 1995 | A |
| 5585658 | Mukai et al. | Dec 1996 | A |
| 6004864 | Huang | Dec 1999 | A |
| 6261964 | Wu | Jul 2001 | B1 |
| 6326300 | Liu et al. | Dec 2001 | B1 |
| 9934982 | Prasad et al. | Apr 2018 | B2 |
| 20080286954 | Kim et al. | Nov 2008 | A1 |
| 20130288471 | Chi | Oct 2013 | A1 |
| 20160276465 | Hung et al. | Sep 2016 | A1 |
| 20170178914 | Prasad et al. | Jun 2017 | A1 |
| Number | Date | Country | |
|---|---|---|---|
| 20180182636 A1 | Jun 2018 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 14975968 | Dec 2015 | US |
| Child | 15900989 | US |