Tungsten nitride atomic layer deposition processes

Abstract
In one embodiment, a method for forming a tungsten barrier material on a substrate is provided which includes depositing a tungsten layer on a substrate during a vapor deposition process and exposing the substrate sequentially to a tungsten precursor and a nitrogen precursor to form a tungsten nitride layer on the tungsten layer. Some examples provide that the tungsten layer may be deposited by sequentially exposing the substrate to the tungsten precursor and a reducing gas (e.g., diborane or silane) during an atomic layer deposition process. The tungsten layer may have a thickness of about 50 Å or less and tungsten nitride layer may have an electrical resistivity of about 380 μΩ-cm or less. Other examples provide that a tungsten bulk layer may be deposited on the tungsten nitride layer by a chemical vapor deposition process.
Description
BACKGROUND OF THE INVENTION

1. Field of the Invention


Embodiments of the present invention relate to a method for manufacturing integrated circuit devices. More particularly, embodiments of the invention relate to forming stoichiometric tungsten nitride films using cyclic or atomic layer deposition.


2. Description of the Related Art


Semiconductor device geometries have dramatically decreased in size since such devices were first introduced several decades ago and are continually decreasing in size today. Metal gates made of tungsten are becoming important because of the resistance requirements of these smaller devices. Tungsten is a desirable material because it is widely available and has a lower resistivity and lower contact resistance compared to other conductive metals.


One drawback to using tungsten in a metal gate, however, is that a barrier layer is typically required between silicon and the tungsten to prevent the formation of tungsten silicide. Tungsten silicide has a higher resistivity than tungsten and thus, increases the overall resistance of the gate. Barrier layers, however, also increase the resistance of the device and are deposited in amounts greater than needed due to the inherent limitations of conventional deposition techniques.


Bulk deposition processes, such as physical vapor deposition (PVD) and chemical vapor deposition (CVD), are conventionally used to deposit barrier layers. Bulk deposition processes are high deposition rate processes that maintain certain deposition conditions for a period of time to deposit material having a desired thickness, typically greater than 1,000 Å. This time period varies depending on the dynamics of the reaction and can be complicated where a reaction condition must be maintained for a brief period of time in order to deposit a controllable and repeatable thin layer of material.


There is a need, therefore, for new methods for depositing controllable, repeatable, and thin barrier layers.


SUMMARY OF THE INVENTION

Embodiments of the invention include a method for forming a tungsten nitride layer by alternately pulsing a tungsten-containing compound and a nitrogen-containing compound until a tungsten nitride layer having a thickness of about 100 Å or less is formed.


Embodiments of the invention also include a method for forming a tungsten layer comprising depositing a tungsten nitride barrier layer by alternately pulsing a first tungsten-containing compound and a nitrogen-containing compound, and depositing a tungsten layer by alternately pulsing a second tungsten-containing compound and a reducing compound.


Embodiments of the invention further include a method for forming a tungsten layer, comprising depositing a tungsten nitride barrier layer by alternately pulsing a first tungsten-containing compound and a nitrogen-containing compound, and depositing a tungsten layer on the barrier layer. In one aspect, the tungsten layer is deposited by chemical vapor deposition or physical vapor deposition techniques. In another aspect, the tungsten layer is deposited by alternately pulsing a second tungsten-containing compound and a reducing compound. In yet another aspect, the tungsten layer is deposited by alternately pulsing the second tungsten-containing compound and the reducing compound to form a pre-layer having a thickness of about 50 Å or less followed by bulk tungsten deposition using chemical vapor deposition or physical vapor deposition.





BRIEF DESCRIPTION OF THE DRAWINGS

So that the manner in which the above recited features of the present invention are attained and can be understood in detail, a more particular description of the invention, briefly summarized above, may be had by reference to the embodiments thereof which are illustrated in the appended drawings.


It is to be noted, however, that the appended drawings illustrate only typical embodiments of this invention and are therefore not to be considered limiting of its scope, for the invention may admit to other equally effective embodiments.



FIG. 1 depicts a schematic cross-sectional view of a process chamber that can be used to practice embodiments described herein.



FIG. 2 illustrates a process sequence for the formation of a tungsten nitride barrier layer using a cyclical deposition technique according to one embodiment described herein.



FIG. 3 illustrates a process sequence for the formation of a tungsten nitride layer using a cyclical deposition technique according to another embodiment described herein.



FIG. 4 illustrates a process sequence for the formation of a tungsten nitride layer using a cyclical deposition technique according to another embodiment described herein.



FIG. 4A illustrates a process sequence for the formation of a tungsten nitride layer particularly on a silicon surface using a cyclical deposition technique according to another embodiment described herein.



FIG. 5 shows a cross sectional view of an exemplary metal oxide gate device 10 utilizing a tungsten nitride layer according to the present invention.



FIG. 6 shows a cross sectional view of a conventional DRAM device utilizing a tungsten nitride layer deposited according to an embodiment of a cyclical deposition technique described herein.



FIG. 7 shows an Auger profile showing the atomic concentration of the deposited tungsten nitride layer.





DETAILED DESCRIPTION

A tungsten nitride layer (WxNy) having a thickness less than 100 Å, such as about 20 Å or less, is formed using embodiments of a cyclical deposition technique described herein. The tungsten nitride layer has a resistivity of about 380 μΩ-cm or less, and provides excellent barrier properties for various device applications, such as an electrode in either DRAM or capacitors for example, without subsequent thermal treatment. The tungsten nitride layer also has a significantly reduced fluorine concentration compared to tungsten nitride layers deposited by conventional bulk deposition techniques, such as plasma enhanced chemical vapor deposition (PECVD). The tungsten nitride layer is particularly useful for devices having dimensions of 0.15 microns or less, such as 100 nm (nanometers).


“Cyclical deposition” as used herein refers to the sequential introduction of two or more reactive compounds to deposit a mono layer of material on a substrate surface. The two or more reactive compounds are sequentially introduced into a reaction zone of a processing chamber. Each reactive compound is separated by a delay/pause to allow each compound to adhere and/or react on the substrate surface. In one aspect, a first precursor or compound A is dosed/pulsed into the reaction zone followed by a first time delay/pause. Next, a second precursor or compound B is dosed/pulsed into the reaction zone followed by a second delay. The reactive compounds are alternatively pulsed until a desired film or film thickness is formed on the substrate surface.


In one aspect, a tungsten nitride layer is deposited on a substrate surface by alternately adsorbing a tungsten-containing compound and a nitrogen-containing compound on a substrate surface. The term “compound” is intended to include one or more precursors, reductants, reactants, and catalysts. Each compound may be a single compound or a mixture/combination of two or more compounds. During deposition, the substrate should be maintained at a temperature of about 550° C. or more, such as between 550° C. and 700° C., at a process chamber pressure of between about 1 Torr and about 10 Torr. The tungsten-containing compound is introduced to the substrate surface at a rate between about 1 sccm (standard cubic centimeters per minute) and about 400 sccm, such as between about 10 sccm and about 100 sccm, and pulsed for about 1 second or less, such as about 0.2 seconds or less. The nitrogen-containing compound is introduced to the substrate surface at a rate between about 5 sccm to about 150 sccm, such as between about 5 sccm and about 25 sccm, and thereafter pulsed for about 1 second or less, such as about 0.2 seconds or less. In one aspect, argon is continuously provided as a carrier/purge gas at a rate between about 250 sccm and about 1,000 sccm, such as between about 500 sccm and about 750 sccm. Each cycle, consisting of a pulse of the tungsten-containing compound and a pulse of the nitrogen-containing compound, forms between about 2 Å to about 3 Å of tungsten nitride, such as about 2.5 Å.


A “substrate surface”, as used herein, refers to any substrate surface upon which film processing is performed. For example, a substrate surface may include silicon, silicon oxide, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal alloys, and other conductive materials, depending on the application. A substrate surface may also include dielectric materials such as silicon dioxide and carbon doped silicon oxides.



FIG. 1 illustrates a schematic, partial cross section of an exemplary processing chamber 16 useful for depositing a tungsten nitride layer according to each of the embodiments of the present invention. Such a processing chamber 16 is available from Applied Materials, Inc. located in Santa Clara, Calif., and a brief description thereof follows. A more detailed description may be found in commonly assigned U.S. Ser. No. 10/016,300, filed on Dec. 12, 2001, and issued as U.S. Pat. No. 6,878,206, which is incorporated herein by reference.


The processing chamber 16 may be integrated into an integrated processing platform, such as an Endura SL platform also available from Applied Materials, Inc. Details of the Endura SL platform are described in commonly assigned U.S. Ser. No. 09/451,628, entitled “Integrated Modular Processing Platform,” filed on Nov. 30, 1999, which is incorporated herein by reference.


Referring to FIG. 1, the processing chamber 16 includes a chamber body 14, a lid assembly 20 for gas delivery, and a thermally controlled substrate support member 46. The thermally controlled substrate support member 46 includes a wafer support pedestal 48 connected to a support shaft 48a. The thermally controlled substrate support member 46 may be moved vertically within the chamber body 14 so that a distance between the support pedestal 48 and the lid assembly 20 may be controlled. An example of a lifting mechanism for the support pedestal 48 is described in detail in U.S. Pat. No. 5,951,776, which is hereby incorporated by reference in its entirety.


The support pedestal 48 includes an embedded thermocouple 50a that may be used to monitor the temperature thereof. For example, a signal from the thermocouple 50a may be used in a feedback loop to control power applied to a heater element 52a by a power source 52. The heater element 52a may be a resistive heater element or other thermal transfer device disposed in or in contact with the pedestal 48 utilized to control the temperature thereof. Optionally, the support pedestal 48 may be heated using a heat transfer fluid (not shown).


The support pedestal 48 may be formed from any process-compatible material, including aluminum nitride and aluminum oxide (Al2O3 or alumina) and may also be configured to hold a substrate thereon employing a vacuum, i.e., support pedestal 48 may be a vacuum chuck. Using a vacuum check, the support pedestal 48 may include a plurality of vacuum holes (not shown) that are placed in fluid communication with a vacuum source routed through the support shaft 48a.


The chamber body 14 includes a liner assembly 54 having a cylindrical portion and a planar portion. The cylindrical portion and the planar portion may be formed from any suitable material such as aluminum, ceramic and the like. The cylindrical portion surrounds the support pedestal 48. The cylindrical portion also includes an aperture 60 that aligns with the slit valve opening 44 disposed a sidewall 14b of the housing 14 to allow entry and egress of substrates from the chamber 16.


The planar portion of the liner assembly 54 extends transversely to the cylindrical portion and is disposed against a chamber bottom 14a of the chamber body 14. The liner assembly 54 defines a chamber channel 58 between the chamber body 14 and both the cylindrical portion and planar portion of the liner assembly 54. Specifically, a first portion of channel 58 is defined between the chamber bottom 14a and planar portion of the liner assembly 54. A second portion of channel 58 is defined between the sidewall 14b of the chamber body 14 and the cylindrical portion of the liner assembly 54. A purge gas is introduced into the channel 58 to minimize unwanted deposition on the chamber walls and to control the rate of heat transfer between the chamber walls and the liner assembly 54.


The chamber body 14 also includes a pumping channel 62 disposed along the sidewalls 14b thereof. The pumping channel 62 includes a plurality of apertures, one of which is shown as a first aperture 62a. The pumping channel 62 includes a second aperture 62b that is coupled to a pump system 18 by a conduit 66. A throttle valve 18a is coupled between the pumping channel 62 and the pump system 18. The pumping channel 62, the throttle valve 18a, and the pump system 18 control the amount of gas flow from the processing chamber 16. The size, number, and position of the apertures 62a in communication with the chamber 16 are configured to achieve uniform flow of gases exiting the lid assembly 20 over the support pedestal 48 having a substrate disposed thereon.


The lid assembly 20 includes a lid plate 20a having a gas manifold 34 mounted thereon. The lid plate 20a provides a fluid tight seal with an upper portion of the chamber body 14 when in a closed position. The gas manifold 34 includes a plurality of control valves 32c (only one shown) to provide rapid and precise gas flow with valve open and close cycles of less than about one second, and in one embodiment, of less than about 0.1 seconds. The valves 32c are surface mounted, electronically controlled valves. One valve that may be utilized is available from Fujikin of Japan as part number FR-21-6.35 UGF-APD. Other valves that operate at substantially the same speed and precision may also be used.


The lid assembly 20 further includes a plurality of gas sources 68a, 68b, 68c, each in fluid communication with one of the valves 32c through a sequence of conduits (not shown) formed through the chamber body 14, lid assembly 20, and gas manifold 34.


The processing chamber 16 further includes a reaction zone 100 that is formed within the chamber body 14 when the lid assembly 20 is in a closed position. Generally, the reaction zone 100 includes the volume within the processing chamber 16 that is in fluid communication with a wafer 102 disposed therein. The reaction zone 100, therefore, includes the volume downstream of each valve 32c within the lid assembly 20, and the volume between the support pedestal 48 and the lower surface of the lid plate 20. More particularly, the reaction zone 100 includes the volume between the outlet of the dosing valves 32c and an upper surface of the wafer 102.


A controller 70 regulates the operations of the various components of the processing chamber 16. The controller 70 includes a processor 72 in data communication with memory, such as random access memory 74 and a hard disk drive 76 and is in communication with at least the pump system 18, the power source 52, and the valve 32c.


Software routines are executed to initiate process recipes or sequences. The software routines, when executed, transform the general purpose computer into a specific process computer that controls the chamber operation so that a chamber process is performed. For example, software routines may be used to precisely control the activation of the electronic control valves for the execution of process sequences according to the present invention. Alternatively, the software routines may be performed in hardware, as an application specific integrated circuit or other type of hardware implementation, or a combination of software or hardware.


Barrier Layer Formation



FIG. 2 illustrates a process sequence 200 for depositing a tungsten nitride layer according to one embodiment of the present invention. As shown in step 202, a substrate is provided to the process chamber. The process chamber conditions, such as the temperature and pressure, for example, are adjusted to enhance the adsorption of the process gases on the substrate. The substrate should be maintained at a temperature of about 550° C. or more, such as between 550° C. and 700° C., at a process chamber pressure of between about 1 Torr and about 10 Torr.


A constant carrier gas stream is established within the process chamber as indicated in step 204. Carrier gases may be selected to also act as a purge gas for the removal of volatile reactants and/or by-products from the process chamber. Carrier gases such as, for example, helium (He), argon (Ar), nitrogen (N2), hydrogen (H2), among others, and combinations thereof may be used. In one aspect, argon is continuously provided at a rate between about 250 sccm and about 1,000 sccm, such as between about 500 sccm and about 750 sccm.


Referring to step 206, after the carrier gas stream is established within the process chamber, a pulse of a tungsten-containing compound is added to the carrier gas stream. A “dose/pulse” as used herein is intended to refer to a quantity of a particular compound that is intermittently or non-continuously introduced into a reaction zone of a processing chamber. The quantity of a particular compound within each pulse may vary over time, depending on the duration of the pulse.


The duration of the pulse of the tungsten-containing compound is variable depending upon a number of factors such as, for example, the volume capacity of the process chamber employed, the vacuum system coupled thereto, and the volatility/reactivity of the particular precursor itself. For example, the tungsten-containing compound is introduced to the substrate surface at a rate between about 1 sccm (standard cubic centimeters per minute) and about 400 sccm, such as between about 10 sccm and about 100 sccm, and pulsed for about 1 second or less, such as about 0.2 seconds or less. More generally, the process conditions are advantageously selected so that a pulse of tungsten-containing compound provides a sufficient amount of volume to absorb at least a monolayer of the tungsten-containing material on the substrate. Thereafter, excess tungsten-containing compound remaining in the chamber is removed from the process chamber by the constant carrier gas stream in combination with the vacuum system.


In step 208, a pulse of a nitrogen-containing compound is added to the carrier gas stream after the excess tungsten-containing compound has been removed from the process chamber. The pulse of nitrogen-containing compound also lasts for a predetermined time that is variable depending upon a number of factors such as, for example, the volume capacity of the process chamber employed, the vacuum system coupled thereto and the volatility/reactivity of the particular precursor itself. For example, the nitrogen-containing compound is introduced to the substrate surface at a rate between about 5 sccm to about 150 sccm, such as between about 5 sccm and about 25 sccm, and thereafter pulsed for about 1 second or less, such as about 0.2 seconds or less. More generally, the duration of the pulse of nitrogen-containing compound should be long enough to adsorb at least a monolayer of the nitrogen-containing compound on the tungsten-containing material. Thereafter, excess nitrogen-containing compound remaining in the chamber is removed by the constant carrier gas stream in combination with the vacuum system.


The duration of each of the pulses of tungsten-containing compound and nitrogen-containing compound may also vary depending on the device geometry, the desired stoichiometry of the deposited layer, and the application of the deposited layer, for example. In one aspect, the duration of the pulse of tungsten-containing compound may be identical to the duration of the pulse of nitrogen-containing compound. In another aspect, the duration of the pulse of tungsten-containing compound may be shorter than the duration of the pulse of nitrogen-containing compound. In still another aspect, the duration of the pulse of tungsten-containing compound may be longer than the duration of the pulse of nitrogen-containing compound.


Additionally, the delays between each pulse of tungsten-containing compound and each pulse of nitrogen-containing compound may have the same duration. That is the duration of the period of non-pulsing between each pulse of the tungsten-containing compound and each pulse of the nitrogen-containing compound can be identical. For such an embodiment, a time interval of non-pulsing between the pulse of the tungsten-containing compound and the pulse of the nitrogen-containing compound is equal to a time interval of non-pulsing between the pulse of the nitrogen-containing compound and the pulse of the tungsten-containing precursor. During the time periods of non-pulsing only the constant carrier gas stream is provided to the process chamber.


The delays between each pulse of tungsten-containing compound and each pulse of nitrogen-containing compound may also have different durations. For example, the duration of the period of non-pulsing between each pulse of the tungsten-containing compound and each pulse of the nitrogen-containing compound may be shorter or longer than the duration of the period of non-pulsing between each pulse of the nitrogen-containing compound and the tungsten-containing precursor. For such an embodiment, a time interval of non-pulsing between the pulse of the tungsten-containing compound and the pulse of the nitrogen-containing compound is different from a time interval of non-pulsing between the pulse of the nitrogen-containing compound and the pulse of the tungsten-containing precursor. During the time periods of non-pulsing, only the constant carrier gas stream is provided to the process chamber.


Additionally, the time intervals for each pulse of the tungsten-containing precursor, the nitrogen-containing compound and the periods of non-pulsing therebetween for each deposition cycle may have the same duration. For such an embodiment, a time interval (T1) for the tungsten-containing precursor, a time interval (T2) for the nitrogen-containing compound, a time interval (T3) of non-pulsing between the pulse of the tungsten-containing compound and the pulse of the nitrogen-containing compound and a time interval (T4) of non-pulsing between the pulse of the nitrogen-containing compound and the pulse of the tungsten-containing compound each have the same value for each deposition cycle. For example, in a first deposition cycle (C1), a time interval (T1) for the pulse of the tungsten-containing compound has the same duration as the time interval (T1) for the pulse of the tungsten-containing compound in a second deposition cycle (C2). Similarly, the duration of each pulse of the nitrogen-containing compound and the periods of non-pulsing between the pulse of the tungsten-containing compound and the nitrogen-containing compound in deposition cycle (C1) is the same as the duration of each pulse of the nitrogen-containing compound and the periods of non-pulsing between the pulse of the tungsten-containing compound and the nitrogen-containing compound in deposition cycle (C2), respectively.


Additionally, the time intervals for at least one pulse of tungsten-containing precursor, at least one pulse of nitrogen-containing compound, and the delays therebetween for one or more of the deposition cycles of the tungsten deposition process may have different durations. For such an embodiment, one or more of the time intervals (T1) for the pulses of the tungsten-containing precursor, the time intervals (T2) for the pulses of the nitrogen-containing compound, the time intervals (T3) of non-pulsing between the pulse of the tungsten-containing compound and the pulse of the nitrogen-containing compound and the time intervals (T4) of non-pulsing between the pulse of the nitrogen-containing compound and the pulse of the tungsten-containing compound may have different values for one or more deposition cycles of the tungsten deposition process. For example, in a first deposition cycle (C1), the time interval (T1) for the pulse of the tungsten-containing compound may be longer or shorter than the time interval (T1) for the pulse of the tungsten-containing compound in a second deposition cycle (C2). Similarly, the duration of each pulse of the nitrogen-containing compound and the periods of non-pulsing between the pulse of the tungsten-containing compound and the nitrogen-containing compound in deposition cycle (C1) may be the same or different than the duration of each pulse of the nitrogen-containing compound and the periods of non-pulsing between the pulse of the tungsten-containing compound and the nitrogen-containing compound in deposition cycle (C2), respectively.


Referring to step 210, after each deposition cycle (steps 204 through 208) a thickness of tungsten nitride will be formed on the substrate. Depending on specific device requirements, subsequent deposition cycles may be needed to achieve a desired thickness. As such, steps 206 and 208 can be repeated until the desired thickness for the tungsten nitride layer is achieved. Thereafter, when the desired thickness is achieved the process is stopped as indicated by step 212. About 2 Å to about 3 Å of tungsten nitride, such as about 2.5 Å, are formed per cycle.


Exemplary tungsten-containing precursors for forming such tungsten layers may include tungsten hexafluoride (WF6) and tungsten hexacarbonyl (W(CO)6), among others, as well as a combination thereof.


Exemplary nitrogen-containing compounds may include nitrogen gas (N2), ammonia (NH3), hydrazine (N2H4), monomethyl hydrazine (CH3N2H3), dimethyl hydrazine (C2H6N2H2), t-butyl hydrazine (C4H9N2H3), phenyl hydrazine (C6H5N2H3), 2,2′-azotertbutane ((CH3)6C2N2), ethylazide (C2H5N3), among others, as well as combinations thereof.


In a particular process sequence 300 described with respect to FIG. 3, a tungsten nitride layer is deposited using separate pulses for each of the tungsten-containing compound, the nitrogen-containing compound, and argon. The deposition sequence 300 includes providing a substrate to the process chamber (step 302); heating the substrate to a temperature greater than 550°C., such as between 550°C. and 700°C. at a pressure less than or about 2 Torr (step 304); providing a pulse of tungsten-containing compound (step 306); providing a first pulse of argon (step 308); providing a pulse of nitrogen-containing compound (step 310); providing a second pulse of argon (step 312); and then repeating steps 304 through 312 until a desired thickness of the tungsten nitride layer has been achieved. Thereafter, the process is stopped (step 316) when the desired thickness is achieved. About 2 Å to about 3 Å of tungsten nitride are formed per cycle.


In FIGS. 2-3, the tungsten deposition cycle is depicted as beginning with a pulse of the tungsten-containing compound followed by a pulse of the nitrogen-containing compound. However, the tungsten deposition cycle may start with a pulse of the nitrogen-containing compound followed by a pulse of the tungsten-containing precursor. Regardless of the pulse sequences, each cycle consists of a pulse of the nitrogen-containing compound and a pulse of the tungsten-containing compound, and cycle is repeated until a desired film or film thickness is achieved.



FIG. 4 shows another process sequence 400 particularly useful for depositing a tungsten nitride barrier layer over a silicon surface. In general, a wafer having a silicon surface is exposed to a chlorine-containing compound, such as dichlorosilane (DCS) for example, prior to alternating pulses of a nitrogen-containing compound and a tungsten-containing compound. The DCS pre-treatment step provides a chlorine terminated silicon surface that resists the formation of tungsten silicide during subsequent exposure to a tungsten-containing compound. Tungsten silicide is undesirable because it increases the resistivity and overall contact resistance of the device.


The nitrogen-containing compound is introduced prior to the tungsten-containing compound to prevent the formation of tungsten silicide due to the reaction of tungsten with the silicon surface. It is believed that the nitrogen-containing compound forms one or more atomic layers of SixNy prior to exposure of the tungsten-containing compound. It is then believed that the one or more atomic layers of SixNy react with the tungsten-containing compound to form one or more atomic layers of WSixNy. The one or more atomic layers of WSixNy provide a much more stable device that is resistant to tungsten diffusion/migration. In metal gate applications, for example, tungsten migration is to be avoided because tungsten atoms may diffuse through the polysilicon gate and come into contact with the dielectric layer, thereby shorting the metal gate.


Referring to FIG. 4, the deposition sequence 400 includes providing a substrate to the process chamber (step 402); heating the substrate to a temperature greater than 550° C., such as between 550° C. and 700° C. at a pressure less than or about 2 Torr (step 404); soaking the substrate in DCS for about 5 seconds to about 1 minute (step 406); providing one or more pulses of ammonia (step 408); introducing a continuous carrier gas stream such as argon gas (step 410); providing a pulse of tungsten hexafluoride (step 412); providing a pulse of ammonia (step 414); and then repeating steps 412 through 414 or stopping the deposition process (step 418) depending on whether a desired thickness for the tungsten nitride layer has been achieved (step 416).



FIG. 4A shows an alternative process sequence 450 useful for depositing a tungsten nitride barrier layer over a silicon surface. The sequence 450 includes providing a substrate to the process chamber (step 452); heating the substrate to a temperature greater than 550° C., such as between 550° C. and 700° C. at a pressure less than or about 2 Torr (step 454); soaking the substrate in DCS for about 5 seconds to about 1 minute (step 456); introducing a continuous carrier gas stream such as argon gas (step 458); providing a pulse of ammonia (step 460); providing a pulse of tungsten hexafluoride (step 462); and then repeating steps 460 through 462 or stopping the deposition process (step 466) depending on whether a desired thickness for the tungsten nitride layer has been achieved (step 466).


Tungsten Metal Gate



FIG. 5 shows a cross sectional view of an exemplary metal oxide gate device utilizing a tungsten nitride barrier layer according to the present invention. The device generally includes an exposed gate 510 surrounded by spacers 516 and silicon source/drain areas 520 formed within a substrate surface 512. The spacers 516 typically consist of an oxide, such as SiO2.


The metal gate 510 includes an oxide layer 511, a polysilicon layer 514, a tungsten nitride layer 515, and a tungsten layer 522. The oxide layer 511, such as a SiO2 layer for example, separates the substrate 512 from the polysilicon layer 514. The oxide layer 511 and the polysilicon layer 514 are deposited using conventional deposition techniques.


The tungsten nitride layer 515 is deposited on the polysilicon layer 514 and is deposited using embodiments of a cyclical deposition technique described above with reference to FIGS. 2-4. In a particular embodiment, similar to the sequence described above with reference to FIG. 4, a process sequence for depositing the tungsten nitride layer 515 on the polysilicon layer 514 includes providing a substrate to the process chamber; heating the substrate to a temperature greater than 550° C., such as between 550° C. and 700° C. at a pressure less than or about 2 Torr; soaking the substrate in DCS for about 5 seconds to about 1 minute; providing one or more pulses of ammonia; introducing a continuous carrier gas stream such as argon gas; providing a pulse of tungsten hexafluoride to the reaction zone; providing a pulse of ammonia to the reaction zone; and then repeating the pulses of tungsten hexafluoride and ammonia until a tungsten nitride layer having a thickness less than 100 Å has been formed.


A tungsten layer 522 is then deposited on the tungsten nitride layer 515. Although any metal deposition process, such as conventional chemical vapor deposition or physical vapor deposition for example, may be used, the tungsten layer 522 may be deposited by alternately adsorbing a tungsten-containing compound and a reducing gas, using a cyclical deposition technique similar to one described above with reference to FIGS. 2-4. Suitable tungsten-containing compounds include, for example, tungsten hexafluoride (WF6) and tungsten hexacarbonyl (W(CO)6), among others. Suitable reducing gases include, for example, silane (SiH4), disilane (Si2H6), dichlorosilane (SiCl2H2), borane (BH3), diborane (B2H6), triborane, tetraborane, pentaborane, hexaborane, heptaborane, octaborane, nonaborane, decaborane, and combinations thereof.


One exemplary process of depositing a tungsten layer includes sequentially providing pulses of tungsten hexafluoride and pulses of diborane. The tungsten hexafluoride may be provided to an appropriate flow control valve at a flow rate of between about 10 sccm (standard cubic centimeters per minute) and about 400 sccm, such as between about 20 sccm and about 100 sccm, and thereafter pulsed for about 1 second or less, such as about 0.2 seconds or less. A carrier gas, such as argon, is provided along with the tungsten hexafluoride at a flow rate between about 250 sccm to about 1,000 sccm, such as between about 500 sccm to about 750 sccm. The diborane may be provided to an appropriate flow control valve at a flow rate of between about 5 sccm and about 150 sccm, such as between about 5 sccm and about 25 sccm, and thereafter pulsed for about 1 second or less, such as about 0.2 seconds or less. A carrier gas, such as argon, is provided along with the diborane at a flow rate between about 250 sccm to about 1,000 sccm, such as between about 500 sccm to about 750 sccm. The substrate is maintained at a temperature between about 250° C. and about 350° C. at a chamber pressure between about 1 Torr and about 10 Torr.


A more detailed description of tungsten deposition using a cyclical deposition technique may be found in commonly assigned U.S. Ser. No. 10/016,300, filed on Dec. 12, 2001, and issued as U.S. Pat. No. 6,878,206, and in commonly assigned U.S. Ser. No. 10/082,048, entitled “Deposition Of Tungsten Films For Dynamic Random Access Memory (DRAM) Application,” filed on Feb. 20, 2002, and published as U.S. Pub. No. 2003-0157760, which are both incorporated herein by reference in their entirety.



FIG. 6 shows another exemplary use of a tungsten nitride barrier layer. More particularly, FIG. 6 is a cross sectional view of a conventional DRAM device having a transistor 620 positioned adjacent a top portion of a trench capacitor 630. The access transistor 620 for the DRAM device 610 is positioned adjacent a top portion of the trench capacitor 630. Preferably, the access transistor 620 comprises an n-p-n transistor having a source region 622, a gate region 624, and a drain region 626. The gate region 624 comprises a P− doped silicon epi-layer disposed over the P+ substrate. The source region 622 of the access transistor 620 comprises an N+ doped material disposed on a first side of the gate region 624, and the drain region 626 comprises an N+ doped material disposed on a second side of the gate region 624, opposite the source region 622. The source region 622 is connected to an electrode of the trench capacitor.


The trench capacitor 630 generally comprises a first electrode 632, a second electrode 634 and a dielectric material 636 disposed therebetween. The P+ substrate serves as a first electrode 632 of the trench capacitor 630 and is connected to a ground connection. A trench 638 is formed in the P+ substrate and filled with a heavily doped N+ polysilicon which serves as the second electrode 634 of the trench capacitor 630. The dielectric material 636 is disposed between the first electrode 632 (i.e., P+ substrate) and the second electrode 634 (i.e., N+ polysilicon).


In one aspect, the trench capacitor 630 also includes a first tungsten nitride barrier layer 640 disposed between the dielectric material 636 and the first electrode 632. Preferably, a second tungsten nitride barrier layer 642 is disposed between the dielectric material 636 and the second electrode 634. Alternatively, the barrier layers 640, 642 are a combination film, such as W/WN. The barrier layers 640, 642 are deposited utilizing embodiments of the cyclical deposition techniques described herein.


Although the above-described DRAM device utilizes an n-p-n transistor, a P+ substrate as a first electrode, and an N+ polysilicon as a second electrode of the capacitor, other transistor designs and electrode materials are contemplated by the present invention to form DRAM devices. Additionally, other devices, such as crown capacitors for example, are contemplated by the present invention.


Embodiments of depositing a tungsten nitride barrier layer using cyclical deposition techniques described herein will be further described below in the following non-limiting example.


EXAMPLE

A tungsten nitride barrier layer was deposited within a cyclical deposition chamber similar to the chamber described above with reference to FIG. 2. The tungsten nitride barrier layer was deposited on a polysilicon layer. The barrier layer was deposited at about 680° C. and about 1.5 Torr. Argon was continuously introduced into the chamber at about 500 sccm. Pulses of tungsten hexafluoride and ammonia were alternately pulsed into the processing chamber, and 40 cycles were performed. Each pulse of tungsten hexafluoride had a rate of about 3 sccm and a duration of about 5 seconds. Each pulse of ammonia had a rate of about 300 sccm and a duration of about 20 seconds. The time delay between pulses was about 20 seconds. The deposition rate was about 2.5 Å per minute. The resulting tungsten nitride layer had a thickness of about 350 Å.



FIG. 7 shows an Auger profile showing the atomic concentration of the deposited tungsten nitride layer. It was surprisingly found that the cyclical deposition technique provided a substantially stoichiometric W2N layer without the need for an additional thermal anneal post-treatment. Further, the deposited stoichiometric W2N layer had a significantly reduced fluorine concentration compared to plasma enhanced chemical vapor deposition (PECVD) WN. The measured resistivity of the barrier layer was 380 μΩ-cm, which is about 50 percent less than a comparable low pressure chemical vapor deposition (LPCVD) WN layer and about 60 percent less than a PVD WN layer.


While the foregoing is directed to embodiments of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, and the scope thereof is determined by the claims that follow.

Claims
  • 1. A The method for forming a tungsten barrier material on a substrate, comprising: exposing a substrate to a tungsten precursor to form a tungsten layer thereon, wherein the tungsten precursor is selected from the group consisting of tungsten hexafluoride, tungsten carbonyl, and derivatives thereof;repeatedly exposing the substrate seguentially to the tungsten precursor and a nitrogen precursor to form a tungsten nitride layer on the tungsten layer, wherein the nitrogen precursor is selected from the group consisting of nitrogen gas, ammonia, hydrazine, monomethyl hydrazine, dimethyl hydrazine, t-butyl hydrazine, phenyl hydrazine, 2,2′-azotertbutane, ethylazide, derivatives thereof, and combinations thereof; anddepositing a tungsten bulk layer over the tungsten nitride layer by a chemical vapor deposition process.
  • 2. A method for forming a tungsten barrier material on a substrate, comprising: depositing a tungsten layer on a substrate during a vapor deposition process; andrepeatedly exposing the substrate seguentially to a tungsten precursor and a nitrogen precursor to form a tungsten nitride layer on the tungsten layer, wherein the nitrogen precursor is selected from the group consisting of nitrogen gas, ammonia, hydrazine, monomethyl hydrazine, dimethyl hydrazine, t-butyl hydrazine, phenyl hydrazine, 2,2′-azotertbutane, ethylazide, derivatives thereof, and combinations thereof.
  • 3. The method of claim 2, wherein the nitrogen precursor comprises ammonia.
  • 4. A method for forming a tungsten barrier material on a substrate, comprising: exposing a substrate to a tungsten precursor to form a tungsten layer thereon; andrepeatedly exposing the substrate seguentially to the tungsten precursor and a nitrogen precursor to form a tungsten nitride layer on the tungsten layer, wherein the nitrogen precursor is selected from the group consisting of nitrogen gas, ammonia, hydrazine, monomethyl hydrazine, dimethyl hydrazine, t-butyl hydrazine, phenyl hydrazine, 2,2′-azotertbutane, ethylazide, derivatives thereof, and combinations thereof.
  • 5. A method for forming a tungsten barrier material on a substrate, comprising: exposing a substrate to tungsten hexafluoride to form a tungsten layer thereon; andrepeatedly exposing the substrate sequentially to tungsten hexafluoride and ammonia to form a tungsten nitride layer on the tungsten layer.
  • 6. The method of claim 5, wherein the tungsten nitride layer has an electrical resistivity of about 380 μΩ-cm or less.
  • 7. A method for forming a tungsten barrier material on a substrate, comprising: exposing a substrate to tungsten hexafluoride to form a tungsten layer thereon;repeatedly exposing the substrate sequentially to tungsten hexafluoride and ammonia to form a tungsten nitride layer on the tungsten layer; anddepositing a tungsten bulk layer over the tungsten nitride layer by a chemical vapor deposition process.
  • 8. The method of claim 7, wherein the tungsten nitride layer has an electrical resistivity of about 380 μΩ-cm or less.
  • 9. The method of claim 7, wherein the tungsten layer is deposited by sequentially exposing the substrate to the tungsten hexafluoride and diborane.
  • 10. A method for forming a tungsten barrier material on a substrate, comprising: exposing a substrate to tungsten hexafluoride to form a tungsten layer thereon;exposing the substrate sequentially to tungsten hexafluoride and ammonia to form a tungsten nitride layer on the tungsten layer, wherein the tungsten nitride layer has an electrical resistivity of about 380 μΩ-cm or less; anddepositing a tungsten bulk layer over the tungsten nitride layer.
  • 11. The method of claim 10, wherein the tungsten nitride layer is deposited by repeatedly exposing the substrate sequentially to the tungsten hexafluoride and ammonia.
CROSS-REFERENCE TO RELATED APPLICATIONS

This application is a continuation of U.S. Ser. No. 11/003,020, filed Dec. 1, 2004, and issued as U.S. Pat. No. 7,115.499, which is a continuation of U.S. Ser. No. 10/084,767, filed Feb. 26, 2002, and issued as U.S. Pat. No. 6,833,161, each of which is herein incorporated by reference in its entirety.

US Referenced Citations (378)
Number Name Date Kind
4058430 Suntola et al. Nov 1977 A
4389973 Suntola et al. Jun 1983 A
4413022 Suntola et al. Nov 1983 A
4486487 Skarp Dec 1984 A
4767494 Kobayashi et al. Aug 1988 A
4806321 Nishizawa et al. Feb 1989 A
4813846 Helms Mar 1989 A
4829022 Kobayashi et al. May 1989 A
4834831 Nishizawa et al. May 1989 A
4838983 Schumaker et al. Jun 1989 A
4838993 Aoki et al. Jun 1989 A
4840921 Matsumoto Jun 1989 A
4845049 Sunakawa Jul 1989 A
4859307 Nishizawa et al. Aug 1989 A
4859627 Sunakawa Aug 1989 A
4861417 Mochizuki et al. Aug 1989 A
4876218 Pessa et al. Oct 1989 A
4917556 Stark et al. Apr 1990 A
4927670 Erbil May 1990 A
4931132 Aspnes et al. Jun 1990 A
4951601 Maydan et al. Aug 1990 A
4960720 Shimbo Oct 1990 A
4975252 Nishizawa et al. Dec 1990 A
4993357 Scholz Feb 1991 A
5000113 Wang et al. Mar 1991 A
5013683 Petroff et al. May 1991 A
5028565 Chang et al. Jul 1991 A
5082798 Arimoto Jan 1992 A
5085885 Foley et al. Feb 1992 A
5091320 Aspnes et al. Feb 1992 A
5130269 Kitahara et al. Jul 1992 A
5166092 Mochizuki et al. Nov 1992 A
5173474 Connell et al. Dec 1992 A
5186718 Tepman et al. Feb 1993 A
5205077 Wittstock Apr 1993 A
5225366 Yoder Jul 1993 A
5234561 Randhawa et al. Aug 1993 A
5246536 Nishizawa et al. Sep 1993 A
5250148 Nishizawa et al. Oct 1993 A
5254207 Nishizawa et al. Oct 1993 A
5256244 Ackerman Oct 1993 A
5259881 Edwards et al. Nov 1993 A
5270247 Sakuma et al. Dec 1993 A
5278435 Van Hove et al. Jan 1994 A
5281274 Yoder Jan 1994 A
5286296 Sato et al. Feb 1994 A
5290748 Knuuttila et al. Mar 1994 A
5294286 Nishizawa et al. Mar 1994 A
5296403 Nishizawa et al. Mar 1994 A
5300186 Kitahara et al. Apr 1994 A
5306666 Izumi et al. Apr 1994 A
5311055 Goodman et al. May 1994 A
5316615 Copel May 1994 A
5316793 Wallace et al. May 1994 A
5330610 Eres et al. Jul 1994 A
5336324 Stall et al. Aug 1994 A
5338389 Nishizawa et al. Aug 1994 A
5348911 Jurgensen et al. Sep 1994 A
5374570 Nasu et al. Dec 1994 A
5395791 Cheng et al. Mar 1995 A
5438952 Otsuka Aug 1995 A
5439876 Graf et al. Aug 1995 A
5441703 Jurgensen Aug 1995 A
5443033 Nishizawa et al. Aug 1995 A
5443647 Aucoin et al. Aug 1995 A
5455072 Bension et al. Oct 1995 A
5458084 Thorne et al. Oct 1995 A
5469806 Mochizuki et al. Nov 1995 A
5480818 Matsumoto et al. Jan 1996 A
5483919 Yokoyama et al. Jan 1996 A
5484664 Kitahara et al. Jan 1996 A
5503875 Imai et al. Apr 1996 A
5521126 Okamura et al. May 1996 A
5526044 Sekine et al. Jun 1996 A
5527733 Nishizawa et al. Jun 1996 A
5532511 Nishizawa et al. Jul 1996 A
5540783 Eres et al. Jul 1996 A
5580380 Liu et al. Dec 1996 A
5601651 Watabe Feb 1997 A
5609689 Kato et al. Mar 1997 A
5616181 Yamamoto et al. Apr 1997 A
5637530 Gaines et al. Jun 1997 A
5641984 Aftergut et al. Jun 1997 A
5644128 Wollnik et al. Jul 1997 A
5667592 Boitnott et al. Sep 1997 A
5674786 Turner et al. Oct 1997 A
5693139 Nishizawa et al. Dec 1997 A
5695564 Imahashi Dec 1997 A
5705224 Murota et al. Jan 1998 A
5707880 Aftergut et al. Jan 1998 A
5711811 Suntola et al. Jan 1998 A
5730801 Tepman et al. Mar 1998 A
5730802 Ishizumi et al. Mar 1998 A
5733816 Iyer et al. Mar 1998 A
5747113 Tsai May 1998 A
5749974 Habuka et al. May 1998 A
5788447 Yonemitsu et al. Aug 1998 A
5788799 Steger et al. Aug 1998 A
5796116 Nakata et al. Aug 1998 A
5801634 Young et al. Sep 1998 A
5804488 Shih et al. Sep 1998 A
5807792 Ilg et al. Sep 1998 A
5830270 McKee et al. Nov 1998 A
5834372 Lee Nov 1998 A
5835677 Li et al. Nov 1998 A
5851849 Comizzoli et al. Dec 1998 A
5855675 Doering et al. Jan 1999 A
5855680 Soininen et al. Jan 1999 A
5856219 Naito et al. Jan 1999 A
5858102 Tsai Jan 1999 A
5866213 Foster et al. Feb 1999 A
5866795 Wang et al. Feb 1999 A
5879459 Gadgil et al. Mar 1999 A
5882165 Maydan et al. Mar 1999 A
5882413 Beaulieu et al. Mar 1999 A
5904565 Nguyen et al. May 1999 A
5916365 Sherman Jun 1999 A
5923056 Lee et al. Jul 1999 A
5923985 Aoki et al. Jul 1999 A
5925574 Aoki et al. Jul 1999 A
5928389 Jevtic Jul 1999 A
5942040 Kim et al. Aug 1999 A
5947710 Cooper et al. Sep 1999 A
5972430 DiMeo, Jr. et al. Oct 1999 A
6001669 Gaines et al. Dec 1999 A
6015590 Suntola et al. Jan 2000 A
6015917 Bhandari et al. Jan 2000 A
6025627 Forbes et al. Feb 2000 A
6036773 Wang et al. Mar 2000 A
6042652 Hyun et al. Mar 2000 A
6043177 Falconer et al. Mar 2000 A
6051286 Zhao et al. Apr 2000 A
6062798 Muka May 2000 A
6071808 Merchant et al. Jun 2000 A
6084302 Sandhu Jul 2000 A
6086677 Umotoy et al. Jul 2000 A
6099604 Sandhu Aug 2000 A
6110556 Bang et al. Aug 2000 A
6113977 Soininen et al. Sep 2000 A
6117244 Bang et al. Sep 2000 A
6124158 Dautartas et al. Sep 2000 A
6130147 Major et al. Oct 2000 A
6139700 Kang et al. Oct 2000 A
6140237 Chan et al. Oct 2000 A
6140238 Kitch Oct 2000 A
6143659 Leem Nov 2000 A
6144060 Park et al. Nov 2000 A
6156382 Rajagopalan et al. Dec 2000 A
6158446 Mohindra et al. Dec 2000 A
6174377 Doering et al. Jan 2001 B1
6174809 Kang et al. Jan 2001 B1
6197683 Kang et al. Mar 2001 B1
6200893 Sneh Mar 2001 B1
6203613 Gates et al. Mar 2001 B1
6206967 Mak et al. Mar 2001 B1
6207302 Sugiura et al. Mar 2001 B1
6207487 Kim et al. Mar 2001 B1
6218298 Hoinkis Apr 2001 B1
6248605 Harkonen et al. Jun 2001 B1
6270572 Kim et al. Aug 2001 B1
6271148 Kao et al. Aug 2001 B1
6274484 Tsai et al. Aug 2001 B1
6284646 Leem Sep 2001 B1
6287965 Kang et al. Sep 2001 B1
6291876 Stumborg et al. Sep 2001 B1
6305314 Sneh et al. Oct 2001 B1
6306216 Kim et al. Oct 2001 B1
6316098 Yitzchaik et al. Nov 2001 B1
6326297 Vijayendran Dec 2001 B1
6333260 Kwon Dec 2001 B1
6335280 Van der Jeugd Jan 2002 B1
6342277 Sherman Jan 2002 B1
6348376 Lim et al. Feb 2002 B2
6355561 Sandhu et al. Mar 2002 B1
6358829 Yoon et al. Mar 2002 B2
6368954 Lopatin et al. Apr 2002 B1
6369430 Adetutu et al. Apr 2002 B1
6372598 Kang et al. Apr 2002 B2
6379748 Bhandari et al. Apr 2002 B1
6391785 Satta et al. May 2002 B1
6391803 Kim et al. May 2002 B1
6399491 Jeon et al. Jun 2002 B2
6416822 Chiang et al. Jul 2002 B1
6420189 Lopatin Jul 2002 B1
6423619 Grant et al. Jul 2002 B1
6428859 Chiang et al. Aug 2002 B1
6447933 Wang et al. Sep 2002 B1
6451119 Sneh et al. Sep 2002 B2
6451695 Sneh Sep 2002 B2
6458701 Chae et al. Oct 2002 B1
6468924 Lee et al. Oct 2002 B2
6475276 Elers et al. Nov 2002 B1
6475910 Sneh Nov 2002 B1
6478872 Chae et al. Nov 2002 B1
6482262 Elers et al. Nov 2002 B1
6482733 Raaijmakers et al. Nov 2002 B2
6482740 Soininen et al. Nov 2002 B2
6511539 Raaijmakers Jan 2003 B1
6524952 Srinivas et al. Feb 2003 B1
6534395 Werkhoven et al. Mar 2003 B2
6534404 Danek et al. Mar 2003 B1
6548424 Putkonen Apr 2003 B2
6551929 Kori et al. Apr 2003 B1
6569501 Chiang et al. May 2003 B2
6585823 Van Wijck Jul 2003 B1
6593484 Yasuhara et al. Jul 2003 B2
6596602 Lizuka et al. Jul 2003 B2
6599572 Saanila et al. Jul 2003 B2
6607976 Chen et al. Aug 2003 B2
6620723 Byun et al. Sep 2003 B1
6630201 Chiang et al. Oct 2003 B2
6632279 Ritala et al. Oct 2003 B1
6635965 Lee et al. Oct 2003 B1
6660126 Nguyen et al. Dec 2003 B2
6686271 Raaijmakers et al. Feb 2004 B2
6784096 Chen et al. Aug 2004 B2
6790773 Drewery et al. Sep 2004 B1
6800173 Chiang et al. Oct 2004 B2
6803272 Halliyal et al. Oct 2004 B1
6815285 Choi et al. Nov 2004 B2
6833161 Wang et al. Dec 2004 B2
6838125 Chung et al. Jan 2005 B2
6893915 Park et al. May 2005 B2
6936538 Byun Aug 2005 B2
6958174 Klaus et al. Oct 2005 B1
7115499 Wang et al. Oct 2006 B2
20010000866 Sneh et al. May 2001 A1
20010002280 Sneh May 2001 A1
20010009140 Bondestam et al. Jul 2001 A1
20010009695 Saanila et al. Jul 2001 A1
20010011526 Doering et al. Aug 2001 A1
20010024387 Raaijmakers et al. Sep 2001 A1
20010025979 Kim et al. Oct 2001 A1
20010028924 Sherman Oct 2001 A1
20010029094 Mee-Young et al. Oct 2001 A1
20010031562 Raaijmakers et al. Oct 2001 A1
20010034123 Jeon et al. Oct 2001 A1
20010041250 Werkhoven et al. Nov 2001 A1
20010042799 Kim et al. Nov 2001 A1
20010050039 Park Dec 2001 A1
20010054730 Kim et al. Dec 2001 A1
20010054769 Raiijmakers et al. Dec 2001 A1
20020000598 Kang et al. Jan 2002 A1
20020004293 Soininen et al. Jan 2002 A1
20020007790 Park Jan 2002 A1
20020009544 Hamaguchi et al. Jan 2002 A1
20020016084 Todd Feb 2002 A1
20020019121 Pyo Feb 2002 A1
20020020869 Park et al. Feb 2002 A1
20020021544 Cho et al. Feb 2002 A1
20020031618 Sherman Mar 2002 A1
20020037630 Agarwal et al. Mar 2002 A1
20020041931 Suntola et al. Apr 2002 A1
20020047151 Kim et al. Apr 2002 A1
20020048635 Kim et al. Apr 2002 A1
20020048880 Lee Apr 2002 A1
20020052097 Park May 2002 A1
20020055235 Agarwal et al. May 2002 A1
20020060363 Xi et al. May 2002 A1
20020061612 Sandhu et al. May 2002 A1
20020068458 Chiang et al. Jun 2002 A1
20020073924 Chiang et al. Jun 2002 A1
20020074588 Lee et al. Jun 2002 A1
20020076481 Chiang et al. Jun 2002 A1
20020076507 Chiang et al. Jun 2002 A1
20020076508 Chiang et al. Jun 2002 A1
20020076837 Hujanen et al. Jun 2002 A1
20020081844 Jeon et al. Jun 2002 A1
20020086507 Park et al. Jul 2002 A1
20020090829 Sandhu et al. Jul 2002 A1
20020094689 Park Jul 2002 A1
20020098627 Pomarede et al. Jul 2002 A1
20020104481 Chiang et al. Aug 2002 A1
20020105088 Yang et al. Aug 2002 A1
20020106536 Lee et al. Aug 2002 A1
20020106846 Seutter et al. Aug 2002 A1
20020109168 Kim et al. Aug 2002 A1
20020115886 Yasuhara et al. Aug 2002 A1
20020117399 Chen et al. Aug 2002 A1
20020121241 Nguyen et al. Sep 2002 A1
20020121342 Nguyen et al. Sep 2002 A1
20020121697 Marsh Sep 2002 A1
20020135071 Kang et al. Sep 2002 A1
20020144655 Chiang et al. Oct 2002 A1
20020144657 Chiang et al. Oct 2002 A1
20020146511 Chiang et al. Oct 2002 A1
20020155722 Satta et al. Oct 2002 A1
20020162506 Sneh et al. Nov 2002 A1
20020164421 Chiang et al. Nov 2002 A1
20020164423 Chiang et al. Nov 2002 A1
20020177282 Song et al. Nov 2002 A1
20020182320 Leskela et al. Dec 2002 A1
20020187256 Elers et al. Dec 2002 A1
20020187631 Kim et al. Dec 2002 A1
20020197402 Chiang et al. Dec 2002 A1
20020197863 Mak et al. Dec 2002 A1
20030013300 Byun Jan 2003 A1
20030013320 Kim et al. Jan 2003 A1
20030017697 Choi et al. Jan 2003 A1
20030031807 Elers et al. Feb 2003 A1
20030032281 Werkhoven et al. Feb 2003 A1
20030038369 Layadi et al. Feb 2003 A1
20030042630 Babcoke et al. Mar 2003 A1
20030049931 Byun et al. Mar 2003 A1
20030049942 Haukka et al. Mar 2003 A1
20030053799 Lei Mar 2003 A1
20030054631 Raaijmakers et al. Mar 2003 A1
20030057526 Chung et al. Mar 2003 A1
20030057527 Chung et al. Mar 2003 A1
20030059538 Chung et al. Mar 2003 A1
20030072884 Zhang et al. Apr 2003 A1
20030072975 Shero et al. Apr 2003 A1
20030079686 Chen et al. May 2003 A1
20030082296 Elers et al. May 2003 A1
20030082300 Todd et al. May 2003 A1
20030082301 Chen et al. May 2003 A1
20030082307 Chung et al. May 2003 A1
20030086111 Akiyoshi May 2003 A1
20030089308 Raaijmakers May 2003 A1
20030101927 Raaijmakers et al. Jun 2003 A1
20030104126 Fang et al. Jun 2003 A1
20030106490 Jallepally et al. Jun 2003 A1
20030108674 Chung et al. Jun 2003 A1
20030116087 Nguyen et al. Jun 2003 A1
20030121608 Chen et al. Jul 2003 A1
20030123216 Yoon et al. Jul 2003 A1
20030124262 Chen et al. Jul 2003 A1
20030129826 Werkhoven et al. Jul 2003 A1
20030134508 Raaijmakers et al. Jul 2003 A1
20030143328 Chen et al. Jul 2003 A1
20030143839 Raaijmakers et al. Jul 2003 A1
20030143841 Yang et al. Jul 2003 A1
20030153181 Yoon et al. Aug 2003 A1
20030157760 Xi et al. Aug 2003 A1
20030161952 Wang et al. Aug 2003 A1
20030165615 Aaltonen et al. Sep 2003 A1
20030168750 Basceri et al. Sep 2003 A1
20030173586 Moriwaki et al. Sep 2003 A1
20030186495 Saanila et al. Oct 2003 A1
20030190423 Yang et al. Oct 2003 A1
20030190497 Yang et al. Oct 2003 A1
20030190804 Yasuda et al. Oct 2003 A1
20030194493 Chang et al. Oct 2003 A1
20030194825 Law et al. Oct 2003 A1
20030203616 Chung et al. Oct 2003 A1
20030205729 Basceri et al. Nov 2003 A1
20030213987 Basceri et al. Nov 2003 A1
20030219942 Choi et al. Nov 2003 A1
20030224217 Byun et al. Dec 2003 A1
20030224578 Chung et al. Dec 2003 A1
20030224600 Cao et al. Dec 2003 A1
20030232497 Xi et al. Dec 2003 A1
20040005749 Choi et al. Jan 2004 A1
20040009307 Koh et al. Jan 2004 A1
20040011504 Ku et al. Jan 2004 A1
20040013577 Ganguli et al. Jan 2004 A1
20040013803 Chung et al. Jan 2004 A1
20040014315 Lai et al. Jan 2004 A1
20040014320 Chen et al. Jan 2004 A1
20040015300 Ganguli et al. Jan 2004 A1
20040018304 Chung et al. Jan 2004 A1
20040018723 Byun et al. Jan 2004 A1
20040018747 Lee et al. Jan 2004 A1
20040033698 Lee et al. Feb 2004 A1
20040041320 Hodumi Mar 2004 A1
20040043630 Vaartstra et al. Mar 2004 A1
20040046197 Basceri et al. Mar 2004 A1
20040077183 Chung et al. Apr 2004 A1
20040187304 Chen et al. Sep 2004 A1
20040219784 Kang et al. Nov 2004 A1
20040224506 Choi et al. Nov 2004 A1
20040235285 Kang et al. Nov 2004 A1
20040256351 Chung et al. Dec 2004 A1
20050006799 Brock et al. Jan 2005 A1
20050009325 Chung et al. Jan 2005 A1
20050059240 Choi et al. Mar 2005 A1
20050104142 Narayanan et al. May 2005 A1
20050176240 Wang et al. Aug 2005 A1
Foreign Referenced Citations (206)
Number Date Country
196 27 017 Jul 1995 DE
198 20 147 Dec 1997 DE
0 344 352 Dec 1989 EP
0 429 270 May 1991 EP
0 442 290 Aug 1991 EP
0 799 641 Oct 1997 EP
1 167 569 Jan 2002 EP
2 626 110 Jul 1989 FR
2 692 597 Dec 1993 FR
2 355 727 May 2001 GB
58-098917 Jun 1983 JP
58-100419 Jun 1983 JP
60-065712 Apr 1985 JP
61-035847 Feb 1986 JP
61-210623 Sep 1986 JP
62-069508 Mar 1987 JP
62-091495 Apr 1987 JP
62-141717 Jun 1987 JP
62-167297 Jul 1987 JP
62-171999 Jul 1987 JP
62-232919 Oct 1987 JP
63-062313 Mar 1988 JP
63-085098 Apr 1988 JP
63-090833 Apr 1988 JP
63-222420 Sep 1988 JP
63-222421 Sep 1988 JP
63-227007 Sep 1988 JP
63-252420 Oct 1988 JP
63-266814 Nov 1988 JP
64-009895 Jan 1989 JP
64-009896 Jan 1989 JP
64-009897 Jan 1989 JP
64-037832 Feb 1989 JP
64-082615 Mar 1989 JP
64-082617 Mar 1989 JP
64-082671 Mar 1989 JP
64-082676 Mar 1989 JP
01-103982 Apr 1989 JP
01-103996 Apr 1989 JP
64-090524 Apr 1989 JP
01-117017 May 1989 JP
01-143221 Jun 1989 JP
01-143233 Jun 1989 JP
01-154511 Jun 1989 JP
01-236657 Sep 1989 JP
01-245512 Sep 1989 JP
01-264218 Oct 1989 JP
01-270593 Oct 1989 JP
01-272108 Oct 1989 JP
01-290221 Nov 1989 JP
01-290222 Nov 1989 JP
01-296673 Nov 1989 JP
01-303770 Dec 1989 JP
01-305894 Dec 1989 JP
01-313927 Dec 1989 JP
02-012814 Jan 1990 JP
02-014513 Jan 1990 JP
02-017634 Jan 1990 JP
02-063115 Mar 1990 JP
02-074029 Mar 1990 JP
02-074587 Mar 1990 JP
02-106822 Apr 1990 JP
02-129913 May 1990 JP
02-162717 Jun 1990 JP
02-172895 Jul 1990 JP
02-196092 Aug 1990 JP
02-203517 Aug 1990 JP
02-230690 Sep 1990 JP
02-230722 Sep 1990 JP
02-246161 Oct 1990 JP
02-264491 Oct 1990 JP
02-283084 Nov 1990 JP
02-304916 Dec 1990 JP
03-019211 Jan 1991 JP
03-022569 Jan 1991 JP
03-023294 Jan 1991 JP
03-023299 Jan 1991 JP
03-044967 Feb 1991 JP
03-048421 Mar 1991 JP
03-070124 Mar 1991 JP
03-185716 Aug 1991 JP
03-208885 Sep 1991 JP
03-234025 Oct 1991 JP
03-286522 Dec 1991 JP
03-286531 Dec 1991 JP
04-031391 Feb 1992 JP
04-031396 Feb 1992 JP
04-100292 Apr 1992 JP
04-111418 Apr 1992 JP
04-132214 May 1992 JP
04-132681 May 1992 JP
04-151822 May 1992 JP
04-162418 Jun 1992 JP
04-175299 Jun 1992 JP
04-186824 Jul 1992 JP
04-212411 Aug 1992 JP
04-260696 Sep 1992 JP
04-273120 Sep 1992 JP
04-285167 Oct 1992 JP
04-291916 Oct 1992 JP
04-325500 Nov 1992 JP
04-328874 Nov 1992 JP
05-029228 Feb 1993 JP
05-047665 Feb 1993 JP
05-047666 Feb 1993 JP
05-047668 Feb 1993 JP
05-074717 Mar 1993 JP
05-074724 Mar 1993 JP
05-102189 Apr 1993 JP
05-160152 Jun 1993 JP
05-175143 Jul 1993 JP
05-175145 Jul 1993 JP
05-182906 Jul 1993 JP
05-186295 Jul 1993 JP
05-206036 Aug 1993 JP
05-234899 Sep 1993 JP
05-235047 Sep 1993 JP
05-251339 Sep 1993 JP
05-270997 Oct 1993 JP
05-283336 Oct 1993 JP
05-291152 Nov 1993 JP
05-304334 Nov 1993 JP
05-343327 Dec 1993 JP
05-343685 Dec 1993 JP
06-045606 Feb 1994 JP
06-132236 May 1994 JP
06-177381 Jun 1994 JP
06-196809 Jul 1994 JP
06-222388 Aug 1994 JP
06-224138 Aug 1994 JP
06-230421 Aug 1994 JP
06-252057 Sep 1994 JP
06-291048 Oct 1994 JP
07-070752 Mar 1995 JP
07-086269 Mar 1995 JP
07-300649 Nov 1995 JP
08-181076 Jul 1996 JP
08-245291 Sep 1996 JP
08-264530 Oct 1996 JP
09-260786 Oct 1997 JP
09-293681 Nov 1997 JP
10-188840 Jul 1998 JP
10-190128 Jul 1998 JP
10-308283 Nov 1998 JP
11-269652 Oct 1999 JP
2000-031387 Jan 2000 JP
2000-058777 Feb 2000 JP
2000-068072 Mar 2000 JP
2000-087029 Mar 2000 JP
2000-138094 May 2000 JP
2000-178735 Jun 2000 JP
2000-218445 Aug 2000 JP
2000-319772 Nov 2000 JP
2000-340883 Dec 2000 JP
2000-353666 Dec 2000 JP
2001-020075 Jan 2001 JP
2001-062244 Mar 2001 JP
2001-111000 Apr 2001 JP
2001-152339 Jun 2001 JP
2001-172767 Jun 2001 JP
2001-189312 Jul 2001 JP
2001-217206 Aug 2001 JP
2001-220287 Aug 2001 JP
2001-220294 Aug 2001 JP
2001-240972 Sep 2001 JP
2001-254181 Sep 2001 JP
2001-284042 Oct 2001 JP
2001-303251 Oct 2001 JP
2001-328900 Nov 2001 JP
WO 9002216 Mar 1990 WO
WO 9110510 Jul 1991 WO
WO 9302111 Feb 1993 WO
WO 9617107 Jun 1996 WO
WO 9618756 Jun 1996 WO
WO 9806889 Feb 1998 WO
WO 9851838 Nov 1998 WO
WO 9901595 Jan 1999 WO
WO 9913504 Mar 1999 WO
WO 9929924 Jun 1999 WO
WO 9941423 Aug 1999 WO
WO 9965064 Dec 1999 WO
WO 0011721 Mar 2000 WO
WO 0015865 Mar 2000 WO
WO 0015881 Mar 2000 WO
WO 0016377 Mar 2000 WO
WO 0054320 Sep 2000 WO
WO 0063957 Oct 2000 WO
WO 0079019 Dec 2000 WO
WO 0079576 Dec 2000 WO
WO 0115220 Mar 2001 WO
WO 0117692 Mar 2001 WO
WO 0127346 Apr 2001 WO
WO 0127347 Apr 2001 WO
WO 0129280 Apr 2001 WO
WO 0129891 Apr 2001 WO
WO 0129893 Apr 2001 WO
WO 0136702 May 2001 WO
WO 0140541 Jun 2001 WO
WO 0166832 Sep 2001 WO
WO 0201628 Jan 2002 WO
WO 0208485 Jan 2002 WO
WO 0245167 Jan 2002 WO
WO 0243115 May 2002 WO
WO 0245871 Jun 2002 WO
WO 0246489 Jun 2002 WO
WO 02067319 Aug 2002 WO
Related Publications (1)
Number Date Country
20070020924 A1 Jan 2007 US
Continuations (2)
Number Date Country
Parent 11003020 Dec 2004 US
Child 11532114 US
Parent 10084767 Feb 2002 US
Child 11003020 US