With the increasing down-scaling of integrated circuits and the increasingly demanding requirements to the speed of integrated circuits, transistors need to have higher drive currents with increasingly smaller dimensions. Fin Field-Effect Transistors (FinFETs) were thus developed. The FinFETs include vertical semiconductor fins. The semiconductor fins are used to form source and drain regions, and to form channel regions between the source and drain regions. Shallow Trench Isolation (STI) regions are formed to define the semiconductor fins. The FinFETs also include gate stacks, which are formed on the sidewalls and the top surfaces of the semiconductor fins.
In the replacement of dummy gates used in a gate-last fabrication, hard mask layer(s) of nitrides and/or oxides may be formed over a dummy gate electrode, such as polysilicon. Replacing the dummy gate can involve etching the hard masks, however, due to gate loading effects gate heights may have different heights and widths. Etching the hard masks may cause shortening of some of the gates, due in part to gate loading and etch rate variations in the etching chamber.
In a plasma etching process, a gas is first introduced into a reaction chamber and then plasma is generated from the gas. This is accomplished by dissociation of the gas into ions, free radicals and electrons by using an RF (radio frequency) generator, which includes one or more electrodes. The electrons are accelerated in an electric field generated by the electrodes, and the energized electrons strike gas molecules to form additional ions, free radicals and electrons, which strike additional gas molecules, and the plasma eventually becomes self-sustaining. The ions, free radicals and electrons in the plasma react chemically with the layer material on the semiconductor wafer to form residual products which leave the wafer surface and, thus, etch the material from the wafer.
Aspects of the present disclosure are best understood from the following detailed description when read with the accompanying figures. It is noted that, in accordance with the standard practice in the industry, various features are not drawn to scale. In fact, the dimensions of the various features may be arbitrarily increased or reduced for clarity of discussion.
The following disclosure provides many different embodiments, or examples, for implementing different features of the invention. Specific examples of components and arrangements are described below to simplify the present disclosure. These are, of course, merely examples and are not intended to be limiting. For example, the formation of a first feature over or on a second feature in the description that follows may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which additional features may be formed between the first and second features, such that the first and second features may not be in direct contact. In addition, the present disclosure may repeat reference numerals and/or letters in the various examples. This repetition is for the purpose of simplicity and clarity and does not in itself dictate a relationship between the various embodiments and/or configurations discussed.
Further, spatially relative terms, such as “beneath,” “below,” “lower,” “above,” “upper” and the like, may be used herein for ease of description to describe one element or feature's relationship to another element(s) or feature(s) as illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The apparatus may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein may likewise be interpreted accordingly.
Embodiments provide temperature control at the edge of a wafer in a dry etch process to provide a more consistent etch rate. In a dry etch process, an electrostatic chuck holds a wafer in a process etching chamber. Etchant gasses are provided in the chamber and a plasma is created by an RF generator and controlled with a voltage bias. A number of factors may affect etch rate at any particular point on the wafer. For example, the location and availability of etchant gasses varies throughout the etch process. Temperature affects etch rate as well. In some instances, etch rate decreases as temperature increases. While the underside of the electrostatic chuck may have cooling pipes, the edge of the wafer overlaps the edge of the electrostatic chuck platform to protect the electrostatic chuck from etchant processes. An insert ring is located at a periphery of the electrostatic chuck and holds the edge of the wafer. As a result of this arrangement, the temperature at the edge of the wafer may be higher than the temperature towards the center of the wafer. During an idle chamber time, the heat retained in the insert ring may transfer to the wafer edge, causing the wafer edge to not cool as quickly as the center of the wafer. As a result when etching resumes, the heat retained in the wafer edge may inhibit etch rate in the wafer edge regions.
When a wafer is etched under such a configuration, the hotter temperature at the edge of the wafer results in a lower etch rate at the edge of the wafer. This is undesirable because extended etching times used to fully etch the edge portions of the wafer may cause interior portions of the wafer to etch more than desired. Also, if the material to be etched is already thicker at the edge of the wafer due to process variations, the problem is further exacerbated and a resulting difference in the height of structures before and after etching may be worse than prior to etching.
As described in detail below, a thermal pad is placed between the insert ring and the electrostatic chuck to dissipate heat from the wafer edge through the insert ring into the electrostatic chuck. As a result, as described below a wafer may be etched in a more consistent manner and provide loading uniformity across multiple structures.
A shadow ring 18 is positioned inside the reaction chamber 20 which can be lifted up to a process position by lifting pins 32. The lifting pins 32 lift the shadow ring 12 away from the wafer 52 when a wafer is being loaded or unloaded. Cooling gas channels 34 are provided inside the electrostatic chuck 16 near its top surface. A high heat conductivity gas such as helium can be circulated through the cooling gas channels 34 to provide a suitable gas on the bottom side of wafer 30 for transferring heat away from the wafer to the electrostatic chuck 16 during an etch process. The electrostatic chuck 16 may also be water cooled which is not shown. The electrostatic chuck 16 is aligned by an electrostatic chuck collar 38. Etching gas is fed into reaction chamber 20 through gas inlets 28. A thermocouple 42 is mounted in the ceiling block 22 for monitoring temperature.
The shadow ring 18 may comprise a ceramic material such as quartz (SiO2) for its high temperature stability. However, when quartz is bombarded by plasma ions, oxygen atoms may release from the quartz and become a contamination hazard. The quartz ring may be topped by a silicon insert ring 48 and by a silicon top collar ring 54 which may alleviate or minimize contamination issues and protect the shadow ring 18 from build-up of etching byproducts.
An insulating ring 50 surrounds the cathode 14 for electrical isolation. Base members 44 and 46 provide platform support.
The magnified call out illustrates a thermal pad 60 positioned between the insert ring (or focus ring) 58 and the electrostatic chuck 16. The thermal pad 60 provides for thermal dissipation from the wafer 52 and insert ring 58 through the thermal pad 60 to the electrostatic chuck 16. Because the electrostatic chuck 16 may have cooling mechanisms built in (e.g., water cooling and/or gas cooling channels), the heat dissipation from the electrostatic chuck 16 can more efficiently be used to dissipate heat from the edge of the wafer 52 and the insert ring 58. The composition and fabrication of the thermal pad will be discussed further below.
One benefit for dissipating heat from the wafer 52 edge, as discussed above, is that the etch rate for devices on the edge of the wafer 52 can be made more uniform to the etch rate for devices in the center of the wafer 52. The etch rate can also be affected by a number of other factors. For example, if the insert ring 58 is made of silicon, plasma etchant can be attracted to the silicon of the insert ring and reduce the etch rate at the edge of the wafer. Accordingly, increasing the etch rate of the edge portions of the wafer 52 by other means is desirable.
In
Modifying insert ring 48 may include mechanically grinding or laser cutting a step out of the bottom side of the insert ring 48 by removing material from the insert ring 48. Other suitable processes may be used to remove material from the insert ring. The dimensions of the step created include a bottom step height D2 and a bottom step width D3. The bottom step height D2 may be selected based on the thickness of the thermal pad 60. The bottom step width D3 may be selected based on the width of the thermal pad 60. The remaining center step height D4 is about equal to the initial step height D1 minus the bottom step height D2. The bottom step width D3 may be about the same or larger than the insert ring 48 step width Do. In some embodiments the bottom step height D2 is between about 0.4 and about 0.6 mm, such as about 0.5 mm. In some embodiments the bottom step width D3 is between about 6 and about 7 mm or between about 6.4 and about 6.5 mm, such as about 6.5 mm. In some embodiments the center step height D4 is between about 3 and about 4 mm or between about 3.4 and about 3.6 mm, such as about 3.5 mm. Other dimensions may be used and generally depend on the dimensions of the electrostatic chuck 16 step.
Thermal pad 60 has a thickness D5 and a width D6. The thickness D5 may correspond to the bottom step height D2. In some embodiments where the thermal pad 60 includes a compressible material or adhesive, the thermal pad 60 may have a thickness D5 which is slightly larger than the bottom step height D2. In some embodiments where the thermal pad 60 does not include a compressible material or adhesive, the thickness D5 may be slightly smaller than the bottom step height D2 to account for a later applied adhesive. The width D6 of the thermal pad 60 may be less than or equal to the bottom step width D3.
The thermal pad 60 may be a conformable material suitable to fill the bottom step of the insert ring 58. The thermal pad 60 may be a thermally conductive material to conduct heat away from the insert ring 58 and wafer 52. In some embodiments, the thermal pad 60 is formed of a silicone-based thermal interface material produced by Shin-Etsu Chemical. These materials may, for example, comprise an elastomer with metallic fillers. Other materials, such as a thermal interface material or a polymer may also be used. In some embodiments, the thermal pad 60 is formed of a silicone resin cast in a mold. In such embodiments, the silicone resin may include a metallic filler to improve thermal conductivity. In some embodiments, the filler material may include a metallic oxide or nitride, such as aluminum oxide, aluminum nitride, copper oxide, beryllium oxide, iron oxide, and so forth. In some embodiments, the filler material may include a metal or composite, such as silver, copper, aluminum, titanium, magnesium, gold, and so forth, or combinations thereof. In some embodiments, the composition of the thermal pad 60 includes carbon, oxygen, aluminum, and silicon.
The thermal pad 60 has a higher thermal conductivity than other elements of the etching chamber 10 which are in contact with the insert ring 58. In some embodiments, the thermal pad 60 has a thermal conductivity between about 4 and 6, such as about 5 W/m·K.
The electrostatic chuck 16 has a step with a height D8 and a width D7. In some embodiments the step height D8 is between about 4.1 and about 4.3 mm, such as about 4.2 mm. In some embodiments the step width D7 is between about 6.55 and about 6.65 mm, such as about 6.6 mm. Other dimensions may be used and generally depend on the dimensions of the electrostatic chuck 16 step.
The thermal pad 60 may comprise a material having a tackiness on its surfaces and can be mounted to either the electrostatic chuck 16 or the insert ring 58. In some embodiments, an adhesive (not shown) can be added to the thermal pad 60 or the mating surface of the electrostatic chuck 16 or insert ring 58 to mount the thermal pad 60. In some embodiments, the adhesive may have thermally conductive characteristics. In some embodiments, the thermal pad 60 may be removed by physical force, such as by peeling or scraping the thermal pad 60 away from the insert ring 58 or electrostatic chuck 16. In some embodiments, an adhesive can be released, such as by exposing the adhesive to a release agent, UV light, or suitable temperature to break down the adhesive, allowing removal of the thermal pad 60.
After mounting the thermal pad 60, the insert ring 58 may be reinstalled and the top collar ring 54 reinstalled.
In
In
In
It should be understood that embodiments of
In some embodiments, the void(s) 61 of
The layers of the dummy gate stacks 201/211/221 may be formed by a progressive deposition of the dummy gate materials and then patterned to form the dummy gates stacks 201/211/221. The dummy gate dielectrics 202/212/222 may be formed from a dummy gate dielectric layer deposited over the semiconductor material 200. The dummy gate dielectric layer may be, for example, silicon oxide, silicon nitride, a combination thereof, or the like, and may be deposited (using, for example, CVD, PVD, a combination thereof, or the like) or thermally grown (for example, using thermal oxidation, or the like) according to acceptable techniques. A dummy gate layer is formed over the dummy dielectric layer, a first hard mask layer formed over the dummy gate layer, and a second hard mask layer formed over the first hard mask layer. In some embodiments, the dummy gate layer may be deposited over the dummy dielectric layer and then planarized using, for example, a CMP process. The dummy gate layer may be between about 80 nm and 120 nm thick (for example, the thickness D11 may be about 95 nm) and may be made of, for example, polysilicon, although other materials may also be used.
The first hard mask layer may be deposited over the dummy gate layer. The second hard mask layer may be deposited over the first hard mask layer. The first hard mask layer and the second hard mask layer may include one or more layers of, for example, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, the like, or a combination thereof, and may be deposited (using, for example, CVD, PVD, a combination thereof, or the like) or thermally grown (for example, using thermal oxidation, or the like) according to acceptable techniques. In an embodiment, the first hard mask layer comprises a layer formed of silicon nitride and the second mask layer comprises a layer formed of silicon oxide. In some embodiments, the first mask layer may have a thickness between about 7 nm and about 13 nm (for example, the thickness D12 may be about 10 nm), and the second mask layer may have a thickness between about 45 nm and about 130 nm (for example, the thickness D13 may be about 50 nm).
The second hard mask layer may be patterned using acceptable photolithography and etching techniques to form the second hard masks 208/218/228. The pattern of the second hard masks 208/218/228 may then be transferred to the first hard mask layer, and dummy gate layer by an acceptable etching technique to form dummy gates 201/211/221. Optionally, the pattern of the second hard masks 208/218/228 may similarly be transferred to dummy dielectric layer (as shown in
A size of dummy gate stacks 201/211/221, and a pitch between the dummy gates stacks 201/211/221, may depend on a region of a die in which the dummy gates stacks 201/211/221 are formed. In some embodiments, dummy gates 201/211/221 may have a larger size and a larger pitch when located in an input/output region of a die (e.g., where input/output circuitry is disposed) than when located in a logic region of a die (e.g., where logic circuitry is disposed). In some embodiments, dummy gates, such as the dummy gates 201/211/221, may have a width between about 15 nm and about 100 nm. In some embodiments, dummy gates, such as the dummy gates 201/211/221, may have a width between about 100 nm and about 300 nm. For example, in
A first gate spacer layer 209 is formed on exposed surfaces of the dummy gates 201/211/221. Any suitable methods of forming the first gate spacer layer 209 may be used. In some embodiments, a deposition (such as CVD, ALD, or the like) or thermal oxidation may be used form the first gate spacer layer 209. In some embodiments, the first gate spacer layer 209 may include one or more layers of, for example, silicon nitride (SiN), silicon oxynitride, silicon carbonitride, silicon oxycarbonitride (SiOCN), a combination thereof, or the like. In some embodiments, a second gate spacer 232 may be formed over the first gate spacer layer 209 using similar processes and materials as the first gate spacer layer 209. In some embodiments, prior to forming the second gate spacer 232, some gates may be masked to prevent formation of the second spacer layer thereon. For example, in
In
During the process to remove lateral portions of the first gate spacer layer 209, due to gate loading variations and etching rate differences associated with process variations, the resulting dummy gate stack 201 may be etched more than the dummy gate stacks 211/221. For example, the dummy gate stack 211 is wider than the dummy gate stack 201. Thus, removing the excess portions of the first gate spacer layer 209 from atop the second hard mask 218 will take longer than removing the excess portions of the first gate spacer layer 209 from atop the second hard mask 208 of the first dummy gate stack 201. As a result, when the first gate spacer layer 209 is anisotropically etched, the portion of the first gate spacer layer 209 over the second hard mask 208 will be removed and the second hard mask 208 may begin to etch while the first gate spacer layer 209 is still being etched from over the second dummy gate stack 211. In the example illustrated in
The third dummy gate stack 221 has a similar width as the first dummy gate stack 201. However, the third dummy gate stack 221 has the second gate spacer 232 deposited thereon, which may act to prevent the selective etching of the lateral portions of first gate spacer layer 209 over the third dummy gate stack 221.
Thus, the gate height of the first dummy gate stack 201 (including the hard masks 206/208, not including the dummy gate dielectric 202) is the height D14, which in some embodiments may be between about 100 nm and 180 nm, for example, about 140 nm. The gate height of the second dummy gate stack 211 (including the hard masks 216/218, not including the dummy gate dielectric 212) is the height D15, which in some embodiments may be between about 135 nm and 215 nm, for example, about 175 nm. The gate height of the third dummy gate stack 221 (including the hard masks 226/228 and first gate spacer 230 and second gate spacer 232, not including the dummy gate dielectric 222) is the height D16, which in some embodiments may be between about 150 nm and 250 nm, for example, about 200 nm. However, these dimensions are merely examples and any suitable dimensions may be utilized.
Referring to
The epitaxial source/drain structures 240 may be doped in situ during formation or doped after formation with an appropriate n-type or p-type dopant.
As discussed above, the semiconductor material 200 may correspond to the wafer 52 of
Due to the gate loading effects (for example, dummy gate stack 211 being wider than dummy gate stack 201 or dummy gate stack 201 being shorter than dummy gate stack 221), there may be different etch rates across the wafer 200. In addition, because the etching may be performed in multiple stages, a chamber idle time may affect the etch rates. For example, a first stage etch may include etching lateral portions of the second gate spacer 232 over dummy gate stack 221 (and like gates). A second stage etch may include etching the remaining lateral portions of the first gate spacer 230 over dummy gate stack 221 (and like gate stacks) which were previously covered by the second gate spacer 232. A third stage etch may include etching the second hard masks 208/218/228 from each of the dummy gate stacks 201/211/221, respectively. A fourth stage etch may include etching the first hard masks 206/216/226 from each of the dummy gate stacks 201/211/221, respectively.
Each of the etching stages may target a particular material for etching, such as various hard masks, however, other non-targeted materials may also be consumed in part or in whole by the etching stages. For example, the photoresist 250 may be consumed by the etching stages. In another example, the first stage etching targeting the second gate spacer 232 may incidentally etch portions of the second hard masks 208 and 218 of the dummy gate stacks 201/211, respectively. Similarly, etching the first gate spacer 230 may incidentally etch portions of the second hard masks 208 and 218 and/or portions of the first hard masks 206 and 216.
In some embodiments, a multistage etch may have a chamber idle time between each stage. Chamber idle time, for example, may be used to clean and maintain the chamber, exchange process gasses, or to allow the chamber to cool between etch stages. As chamber idle time increases, the etch rates upon resumption of etching may increase due to the falling temperature.
A thermal pad, such as the thermal pad 60, provides a continuous heat dissipation mechanism for the wafer edge and insert ring during chamber idle time. The thermal pad 60 allows for a more stable etch rate across the wafer due to better temperature uniformity. Without the thermal pad 60, during chamber idle the edge of the wafer 200 would become disproportionately hot compared to the cooling center portions of the wafer 200. Such disproportionate heat would cause a slow etch rate at those hotter temperatures at the wafer edge and may exacerbate the effect of gate loading differences on gate height. With such differences, narrower gates more susceptible to etchant may become too short and cause gate shorting. With the thermal pad 60, however, due to a more consistent etch rate across the wafer 200 after chamber idle time, the gate height differences due to gate loading effects are improved by making the etch rate more consistent.
A demonstration of the realized effects of the thermal pad 60 will be discussed below, with respect to
Referring to
By using a thermal pad (such as thermal pad 60) in the etching process, the gate height difference in the end device may be less than about 3.0 to about 6.5 nm.
Next, as shown in
Referring to
Next, as shown in
Replacing the dummy gates 201/211/221 with the metal gates 301/311/321 may be done by any suitable process. In some embodiments, the dummy gates 201/211/221 may be removed by etching between the respective first gate spacers 210/220/230 to remove the dummy gate electrodes 205/215/225 and dummy gate dielectrics 202/212/222, using a suitable etchant and etching technique. The dummy gate electrode and dummy gate dielectric removal forms recesses (not shown) between the first gate spacers.
In some embodiments, gate dielectric layers 302/312/322 are deposited conformally in the recesses and over the ILD 260. In some embodiments, the gate dielectric layers 302/312/322 comprise silicon oxide, silicon nitride, or multilayers thereof. In other embodiments, the gate dielectric layers 302/312/322 include a high-k dielectric material, and in these embodiments, the gate dielectric layers 302/312/322 may have a k value greater than about 7.0, and may include a metal oxide or a silicate of Hf, Al, Zr, La, Mg, Ba, Ti, Pb, and combinations thereof. The formation methods of the gate dielectric layers 302/312/322 may include Molecular-Beam Deposition (MBD), ALD, PECVD, a combination thereof, or the like. The gate dielectric layers 302/312/322 may extend over the surface of the ILD 260, which will be removed in a later process.
Next, the gate electrodes 304/314/324 are formed from material deposited over the gate dielectric layers 302/312/322 and fill the remaining portions of the recesses. The gate electrodes 304/314/324 may be made of a metal-containing material such as TiN, TaN, TaC, TiC, TiO, Co, Ru, Al, Ag, Au, W, Ni, Ti, Cu, combinations thereof, or multi-layers thereof. After the filling of the recess with the gate electrode material, a planarization process, such as a CMP, may be performed to remove the excess portions of the gate dielectric layers 302/312/322 and gate electrode material, which excess portions are over the top surface of ILD 260.
Although not illustrated, the gate electrodes 304/314/324 may include a series of one or more stacked layers (not shown). The stacked layers may be deposited conformally in the recesses, over sidewalls and bottoms of the gate electrodes 302/312/322, and over the top surface of the ILD 260. Stacked layers may be formed by a conformal deposition method such as ALD or CVD and have a substantially uniform thickness within process variations. The stacked layers may include a diffusion barrier layer and one or more work function layers over the diffusion barrier layer. The diffusion barrier layer may be formed of titanium nitride (TiN) or thallium nitride. The work function layer(s) determine the work function of the gate, and may include at least one layer, or a plurality of layers formed of different materials. The specific material of the work function layer may be selected according to whether the respective FinFET is an n-type FinFET or a p-type FinFET. For example, when the FinFET is an n-type FinFET, the work function layer may include an AlTiC layer. When the FinFET is a p-type FinFET, the work function layer may include an AlTiN and/or AlTiC layer. After the deposition of the work function layer(s), a barrier layer (not shown), which may be another TiN layer, may be formed. Following the barrier layer, the gate electrode material such as described above can be deposited within the remaining recesses.
In some embodiments, the formation of the gate dielectric layers 302/312/322 may occur simultaneously such that the gate dielectric layers 302/312/322 are made of the same materials, and the formation of the gate electrodes 304/314/324 may occur simultaneously such that the gate electrodes 304/314/324 are made of the same materials. However, in other embodiments, the gate dielectric layers 302/312/322 may be formed by distinct processes, such that the gate dielectric layers 302/312/322 may be made of different materials, and the gate electrodes 304/314/324 may be formed by distinct processes, such that the gate electrodes 304/314/324 may be made of different materials. Various masking steps may be used to mask and expose appropriate regions when using distinct processes.
In some embodiments, the gate electrodes 304/314/324 may be recessed to form second recesses by partially etching the gate electrodes using suitable etchant and etching techniques. A self-aligned contact insulating film may be deposited in the recesses and over the ILD 260. The self-aligned contact insulating film may be made of SiN, silicon oxynitride, silicon carbonitride, SiOCN, a combination thereof, or the like. After forming the self-aligned contact insulating film, a planarization process, such as a CMP, may be performed to remove the excess portions of the self-aligned contact insulating film, which excess portions are over the top surface of ILD 260, thereby forming the self-aligned contact insulating films 306/316/326. In some embodiments, the self-aligned contact insulating films 306/316/326 may be further recessed and a cap layer (not shown) of the same or a different material (such as those listed above for the self-aligned contact insulating film) formed over the self-aligned contact insulating films 306/316/326. The self-aligned contact insulating films 306/316/326 may be used to protect the gates 301/311/321 during formation of self-aligned contacts.
In the illustrated example of
The contact opening 361 over the gate 311 illustrates a self-aligned contact opening that overlaps one gate (the gate 311) but not the adjacent gate (the right gate 301).
As shown in
In
In
As illustrated above in
Referring to
As seen in
In comparison to etch rates without the thermal pad, holding all other factors the same, the etch rates without the thermal pad within three standard deviations (3-sigma) was 4.3 nm±3.7 nm/min to about 4.4 nm±3.5 nm/min, representing a probabilistic etch rate variation of about 164.8% to about 170.6%. The etch rates without the thermal pad had a measured range of 3.8 nm/min to 4.2 nm/min, representing an etch rate variation of 44-49% across measured values.
Table 1 shows a side-by-side comparison of these values.
Thus, the etch rate variation across the wafer is advantageously improved to have less variation when using the thermal pad, such as thermal pad 60.
Referring to
Table 2 shows a side-by-side comparison of the values of
Referring to
Table 3 shows a side-by-side comparison of the values of
Referring to
Table 4 shows a side-by-side comparison of the values of
Without the thermal pad the range for gate height removal (corresponding to Table 4) is 4.39 nm, which is 119.6% of the mean, compared to 2.19 nm, which is 41.6% of the mean, when using the thermal pad. Thus, the gate height variation across the wafer is advantageously improved to have less variation when using the thermal pad, such as thermal pad 60.
Embodiments provide a more consistent etch rate across an entire wafer by using a thermal pad between an insert ring and electrostatic chuck. The thermal pad provides a continuous passive heat path to dissipate heat from the insert ring and wafer edge to the electrostatic chuck. In some embodiments, active cooling mechanism may be located in the electrostatic chuck. The thermal pad helps to keep the temperature of the various components in contact with or near the wafer at a more consistent temperature. Because temperature may affect etch rate, such as with etching hard masks over dummy gate formations, a more consistent etch rate is attained. Further, the benefits of the thermal pad were found to help the etch rate uniformity across the whole wafer and not just at the edge. Embodiments use the thermal pad in an etch process to perform gate replacement by removing hard mask layer(s) over a dummy gate electrode. As a result of using the thermal pad, gate height is better maintained across the etch and gate loading has less impact on gate height. After removal the hard mask, the dummy gate electrodes may be removed and replaced. Contacts can then be formed to the source/drain regions and gate electrodes.
One embodiment is an etching chamber platform that includes an electrostatic chuck, a shadow ring surrounding the electrostatic chuck, and an insert ring on a first inset step of the shadow ring. The insert ring also overlaps an inset step of the electrostatic chuck. The insert ring has a bottom inset step in a portion of the insert ring that overlaps the inset step of the electrostatic chuck. One or more thermal pads are interposed between the insert ring and the electrostatic chuck, where the one or more thermal pads are adjacent to the bottom inset step of the insert ring and the inset step of the electrostatic chuck, the one or more thermal pads having a higher thermal conductivity than the shadow ring.
One embodiment is a method that includes installing a thermal pad into an etching chamber. A stepped insert ring is installed into the etching chamber such that the thermal pad is interposed between the stepped insert ring and an electrostatic chuck of the etching chamber. The thermal pad has a higher thermal conductivity than other elements of the etching chamber in contact with the stepped insert ring.
One embodiment is a method that includes providing etchant gasses in an etching chamber, where the etching chamber has a wafer therein. A plasma is generated the etchant gasses. The plasma is used to etch structures on the wafer. Heat is dissipated from an insert ring of the etching chamber through a thermal pad to an electrostatic chuck of the etching chamber. The thermal pad has a higher heat transfer than other elements of the chamber in contact with the insert ring.
Another embodiment is a device including a wafer chuck. The device also includes an insert ring laterally surrounding the wafer chuck, the insert ring having an edge portion which is over a portion of the wafer chuck. The device also includes a thermal pad disposed between the insert ring and the wafer chuck, an upper surface of the thermal pad having a first interface with the insert ring and a lower surface of the thermal pad having a second interface with the wafer chuck.
Another embodiment is an etching device including an electrostatic chuck having a first portion wider than a second portion, the second portion being configured to support a wafer during an etching process. The etching device also includes an insert ring laterally surrounding the electrostatic chuck and vertically overlapping the first portion of the electrostatic chuck. The etching device further includes one or more thermal pads interposed between the insert ring and the electrostatic chuck, the one or more thermal pads each having a first surface in contact with the insert ring and a second surface in contact with the electrostatic chuck, the one or more thermal pads each being configured to dissipate heat from the insert ring to the electrostatic chuck.
Another embodiment is a device including a thermal pad disposed on a lower ledge of a wafer chuck, the lower ledge surrounding a bottom portion of the wafer chuck. The device also includes an insert ring disposed around the wafer chuck, the insert ring laterally surrounding the wafer chuck, the insert ring contacting an upper surface of the thermal pad, the insert ring having an upper surface level with an upper surface of the wafer chuck.
The foregoing outlines features of several embodiments so that those skilled in the art may better understand the aspects of the present disclosure. Those skilled in the art should appreciate that they may readily use the present disclosure as a basis for designing or modifying other processes and structures for carrying out the same purposes and/or achieving the same advantages of the embodiments introduced herein. Those skilled in the art should also realize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and that they may make various changes, substitutions, and alterations herein without departing from the spirit and scope of the present disclosure.
This application is a divisional of U.S. application Ser. No. 16/266,797, filed on Feb. 4, 2019, which is a continuation of U.S. application Ser. No. 15/726,103, filed on Oct. 5, 2017, now U.S. Pat. No. 10,199,252, issued on Feb. 5, 2019, which claims priority to and the benefit of U.S. Provisional Application No. 62/527,631, filed on Jun. 30, 2017, entitled “Thermal Pad for Etch Rate Uniformity,” which applications are hereby incorporated herein by reference.
| Number | Date | Country | |
|---|---|---|---|
| 62527631 | Jun 2017 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 16266797 | Feb 2019 | US |
| Child | 17360157 | US |
| Number | Date | Country | |
|---|---|---|---|
| Parent | 15726103 | Oct 2017 | US |
| Child | 16266797 | US |