1. Field of the Invention
The present invention relates to a plasma enhanced atomic layer deposition system and a method of operating thereof, and more particularly to a plasma enhanced atomic layer deposition system having reduced contamination.
2. Description of Related Art
Typically, during materials processing, plasma is employed to facilitate the addition and removal of material films when fabricating composite material structures. For example, in semiconductor processing, a (dry) plasma etch process is utilized to remove or etch material along fine trenches or within vias or contacts patterned on a silicon substrate. Alternatively, for example, a vapor deposition process is utilized to deposit material along fine lines or within vias or contacts on a silicon substrate. In the latter, vapor deposition processes include chemical vapor deposition (CVD), and plasma enhanced chemical vapor deposition (PECVD).
In PECVD, plasma is utilized to alter or enhance the film deposition mechanism. For instance, plasma excitation generally allows film-forming reactions to proceed at temperatures that are significantly lower than those typically required to produce a similar film by thermally excited CVD. In addition, plasma excitation may activate film-forming chemical reactions that are not energetically or kinetically favored in thermal CVD. The chemical and physical properties of PECVD films may thus be varied over a relatively wide range by adjusting process parameters.
More recently, atomic layer deposition (ALD), a form of CVD or more generally film deposition, has emerged as a candidate for ultra-thin gate film formation in front end-of-line (FEOL) operations, as well as ultra-thin barrier layer and seed layer formation for metallization in back end-of-line (BEOL) operations. In ALD, two or more process gasses are introduced alternatingly and sequentially in order to form a material film one monolayer at a time. Such an ALD process has proven to provide improved uniformity and control in layer thickness, as well as conformality to features on which the layer is deposited. However, current ALD processes generally have a slow deposition rate that is not feasible for production requirements. Moreover, current ALD processes often suffer from contamination problems that affect the quality of the deposited films, and thus the manufactured device. Factors such as these have been an impediment to wide acceptance of ALD films despite their superior characteristics.
Accordingly, one object of the present invention is directed to addressing any of the above-described and/or other problems with ALD systems and processes.
Another object of the present invention is to reduce contamination problems relating to deposition of ALD films.
These and/or other objects of the present invention may be provided by a method for depositing a film on a substrate using a plasma enhanced atomic layer deposition (PEALD) process. In one aspect, the method includes disposing the substrate in a processing chamber configured to facilitate the PEALD process, introducing a first process material within the processing chamber, and introducing a second process material within the processing chamber. A first level of electromagnetic power is coupled to the processing chamber to generate a plasma that releases contaminants from at least one of a processing chamber component or the substrate, and a second level of electromagnetic power higher than the first level is coupled to the processing chamber during introduction of the second process material to generate a plasma that facilitates a reduction reaction between the first and second process materials at a surface of the substrate.
Another aspect of the present invention includes an atomic layer deposition system having a process chamber, a substrate holder provided within the processing chamber and configured to support a substrate, a first process material supply system configured to supply a first process material to the process chamber and a second process material supply system configured to supply a second process material to the process chamber. Also included is a power source configured to couple a first level of electromagnetic power to the process chamber to generate a plasma that releases contaminants from at least one of a process chamber component or the substrate, and to couple a second level of electromagnetic power higher than the first level to the process chamber during introduction of the second process material to generate a plasma that facilitates a reduction reaction between first and second process materials at a surface of the substrate.
Still another aspect of the invention includes an atomic layer deposition system having a process chamber, means provided within the process chamber for supporting a substrate, means for supplying a first process material to the process chamber and means for supplying a first process material to the process chamber. Also included is means for coupling a first level of electromagnetic power to the process chamber to generate a plasma that releases contaminants from at least one of the process chamber or the substrate. Finally, included is a means for coupling a second level of electromagnetic power higher than the first level to the process chamber during introduction of the second process material to generate a plasma that facilitates a reduction reaction between the first and second process materials at the substrate.
In the accompanying drawings:
FIGS. 9A-C illustrate a substrate zone and a peripheral zone in a PEALD process chamber, and two timing sequences for plasma in the substrate zone and plasma in the peripheral zone according to an embodiment of the present invention;
In the following description, in order to facilitate a thorough understanding of the invention and for purposes of explanation and not limitation, specific details are set forth, such as a particular geometry of the deposition system and descriptions of various components. However, it should be understood that the invention may be practiced in other embodiments that depart from these specific details.
Referring now to the drawings, wherein like reference numerals designate identical or corresponding parts throughout the several views,
The deposition system 1 comprises a process chamber 10 having a substrate holder 20 configured to support a substrate 25, upon which the thin film is formed. The process chamber 10 further comprises an upper assembly 30 coupled to a first process material supply system 40, a second process material supply system 42, and a purge gas supply system 44. Additionally, the deposition system 1 comprises a first power source 50 coupled to the process chamber 10 and configured to generate plasma in the process chamber 10, and a substrate temperature control system 60 coupled to substrate holder 20 and configured to elevate and control the temperature of substrate 25. Additionally, deposition system 1 comprises a controller 70 that can be coupled to process chamber 10, substrate holder 20, upper assembly 30, first process material supply system 40, second process material supply system 42, purge gas supply system 44, first power source 50, and substrate temperature control system 60.
Alternately, or in addition, controller 70 can be coupled to one or more additional controllers/computers (not shown), and controller 70 can obtain setup and/or configuration information from an additional controller/computer.
In
The controller 70 can be used to configure any number of processing elements (10, 20, 30, 40, 42, 44, 50, and 60), and the controller 70 can collect, provide, process, store, and display data from processing elements. The controller 70 can comprise a number of applications for controlling one or more of the processing elements. For example, controller 70 can include a graphic user interface (GUI) component (not shown) that can provide easy to use interfaces that enable a user to monitor and/or control one or more processing elements.
Referring still to
The first process material supply system 40 and the second process material supply system 42 are configured to alternatingly introduce a first process material to process chamber 10 and a second process material to process chamber 10. The alternation of the introduction of the first material and the introduction of the second material can be cyclical, or it may be acyclical with variable time periods between introduction of the first and second process materials. The first process material can, for example, comprise a film precursor, such as a composition having the principal atomic or molecular species found in the film formed on substrate 25. For instance, the film precursor can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 10 in a gaseous phase with or without the use of a carrier gas. The second process material can, for example, comprise a reducing agent, which may also include atomic or molecular species found in the film formed on substrate 25. For instance, the reducing agent can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 10 in a gaseous phase with or without the use of a carrier gas.
Additionally, the purge gas supply system 44 can be configured to introduce a purge gas to process chamber 10. For example, the introduction of purge gas may occur between introduction of the first process material and the second process material to process chamber 10, or following the introduction of the second process material to process chamber 10, respectively. The purge gas can comprise an inert gas, such as a Noble gas (i.e., helium, neon, argon, xenon, krypton), or nitrogen, or hydrogen. In one embodiment, the purge gas supply system 44 can also be configured to introduce a reactive purge gas as will be described below.
Referring still to
Alternatively, the first power source 50 may include a radio frequency (RF) generator and an impedance match network, and may further include an antenna, such as an inductive coil, through which RF power is coupled to plasma in process chamber 10. The antenna can, for example, include a helical or solenoidal coil, such as in an inductively coupled plasma source or helicon source, or it can, for example, include a flat coil as in a transformer coupled plasma source.
Alternatively, the first power source 50 may include a microwave frequency generator, and may further include a microwave antenna and microwave window through which microwave power is coupled to plasma in process chamber 10. The coupling of microwave power can be accomplished using electron cyclotron resonance (ECR) technology, or it may be employed using surface wave plasma technology, such as a slotted plane antenna (SPA), as described in U.S. Pat. No. 5,024,716, entitled “Plasma processing apparatus for etching, ashing, and film-formation”; the contents of which are herein incorporated by reference in its entirety.
Optionally, the plasma generation system includes a first electrode in the upper assembly 30, and a second electrode 30A positioned at a periphery of the upper assembly 30 of deposition system 1′ as shown in
Optionally, the deposition system 1 comprises a substrate bias generation system configured to generate or assist in generating a plasma during at least a portion of the alternating introduction of the first process material and the second process material to process chamber 10. The substrate bias system can include a substrate power source 52 coupled to the process chamber 10, and configured to couple power to substrate 25. The substrate power source 52 may include a radio frequency (RF) generator and an impedance match network, and may further include an electrode through which RF power is coupled to substrate 25. The electrode can be formed in substrate holder 20. For instance, substrate holder 20 can be electrically biased at a RF voltage via the transmission of RF power from a RF generator (not shown) through an impedance match network (not shown) to substrate holder 20. A typical frequency for the RF bias can range from about 0.1 MHz to about 100 MHz. RF bias systems for plasma processing are well known to those skilled in the art. Alternately, RF power is applied to the substrate holder electrode at multiple frequencies.
Although the plasma generation system and the optional substrate bias system are illustrated in
Still referring to
In order to improve the thermal transfer between substrate 25 and substrate holder 20, substrate holder 20 can include a mechanical clamping system, or an electrical clamping system, such as an electrostatic clamping system, to affix substrate 25 to an upper surface of substrate holder 20. Furthermore, substrate holder 20 can further include a substrate backside gas delivery system configured to introduce gas to the back-side of substrate 25 in order to improve the gas-gap thermal conductance between substrate 25 and substrate holder 20. Such a system can be utilized when temperature control of the substrate is required at elevated or reduced temperatures. For example, the substrate backside gas system can comprise a two-zone gas distribution system, wherein the helium gas gap pressure can be independently varied between the center and the edge of substrate 25.
Furthermore, the process chamber 10 is further coupled to a pressure control system 32, including a vacuum pumping system 34 and a valve 36, through a duct 38, wherein the pressure control system 34 is configured to controllably evacuate the process chamber 10 to a pressure suitable for forming the thin film on substrate 25, and suitable for use of the first and second process materials. As seen in
The vacuum pumping systems 34 and 34A can include a turbo-molecular vacuum pump (TMP) or a cryogenic pump capable of a pumping speed up to about 5000 liters per second (and greater) and valve 36 can include a gate valve for throttling the chamber pressure. In conventional plasma processing devices utilized for dry plasma etch, a 300 to 5000 liter per second TMP is generally employed. Moreover, a device for monitoring chamber pressure (not shown) can be coupled to the process chamber 10. The pressure measuring device can be, for example, a Type 628B Baratron absolute capacitance manometer commercially available from MKS Instruments, Inc. (Andover, Mass.).
Still referring to
However, the controller 70 may be implemented as a general-purpose computer system that performs a portion or all of the microprocessor based processing steps of the invention in response to a processor executing one or more sequences of one or more instructions contained in a memory. Such instructions may be read into the controller memory from another computer readable medium, such as a hard disk or a removable media drive. One or more processors in a multi-processing arrangement may also be employed as the controller microprocessor to execute the sequences of instructions contained in main memory. In alternative embodiments, hard-wired circuitry may be used in place of or in combination with software instructions. Thus, embodiments are not limited to any specific combination of hardware circuitry and software.
The controller 70 includes at least one computer readable medium or memory, such as the controller memory, for holding instructions programmed according to the teachings of the invention and for containing data structures, tables, records, or other data that may be necessary to implement the present invention. Examples of computer readable media are compact discs, hard disks, floppy disks, tape, magneto-optical disks, PROMs (EPROM, EEPROM, flash EPROM), DRAM, SRAM, SDRAM, or any other magnetic medium, compact discs (e.g., CD-ROM), or any other optical medium, punch cards, paper tape, or other physical medium with patterns of holes, a carrier wave (described below), or any other medium from which a computer can read.
Stored on any one or on a combination of computer readable media, the present invention includes software for controlling the controller 70, for driving a device or devices for implementing the invention, and/or for enabling the controller to interact with a human user. Such software may include, but is not limited to, device drivers, operating systems, development tools, and applications software. Such computer readable media further includes the computer program product of the present invention for performing all or a portion (if processing is distributed) of the processing performed in implementing the invention.
The computer code devices of the present invention may be any interpretable or executable code mechanism, including but not limited to scripts, interpretable programs, dynamic link libraries (DLLs), Java classes, and complete executable programs. Moreover, parts of the processing of the present invention may be distributed for better performance, reliability, and/or cost.
The term “computer readable medium” as used herein refers to any medium that participates in providing instructions to the processor of the controller 70 for execution. A computer readable medium may take many forms, including but not limited to, non-volatile media, volatile media, and transmission media. Non-volatile media includes, for example, optical, magnetic disks, and magneto-optical disks, such as the hard disk or the removable media drive. Volatile media includes dynamic memory, such as the main memory. Moreover, various forms of computer readable media may be involved in carrying out one or more sequences of one or more instructions to the processor of the controller for execution. For example, the instructions may initially be carried on a magnetic disk of a remote computer. The remote computer can load the instructions for implementing all or a portion of the present invention remotely into a dynamic memory and send the instructions over a network to the controller 70.
The controller 70 may be locally located relative to the deposition system 1 (1′), or it may be remotely located relative to the deposition system 1 (1′). For example, the controller 70 may exchange data with the deposition system 1 (1′) using at least one of a direct connection, an intranet, the Internet and a wireless connection. The controller 70 may be coupled to an intranet at, for example, a customer site (i.e., a device maker, etc.), or it may be coupled to an intranet at, for example, a vendor site (i.e., an equipment manufacturer). Additionally, for example, the controller 70 may be coupled to the Internet. Furthermore, another computer (i.e., controller, server, etc.) may access, for example, the controller 70 to exchange data via at least one of a direct connection, an intranet, and the Internet. As also would be appreciated by those skilled in the art, the controller 70 may exchange data with the deposition system 1 (1′) via a wireless connection.
Referring now to
The deposition system 101 may be configured to process 200 mm substrates, 300 mm substrates, or larger-sized substrates. In fact, it is contemplated that the deposition system may be configured to process substrates, wafers, or LCDs regardless of their size, as would be appreciated by those skilled in the art. Substrates can be introduced to process chamber 110 through passage 112, and they may be lifted to and from an upper surface of substrate holder 120 via substrate lift system 122.
The first process material supply system 140 and the second process material supply system 142 are configured to alternatingly introduce a first process material to process chamber 110 and a second process material to process chamber 110. The alternation of the introduction of the first material and the introduction of the second material can be cyclical, or it may be acyclical with variable time periods between introduction of the first and second materials. The first process material can, for example, comprise a film precursor, such as a composition having the principal atomic or molecular species found in the film formed on substrate 125. For instance, the film precursor can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 10 in a gaseous phase, and with or without a carrier gas. The second process material can, for example, comprises a reducing agent, which may also have atomic or molecular species found in the film formed on substrate 125. For instance, the reducing agent can originate as a solid phase, a liquid phase, or a gaseous phase, and it may be delivered to process chamber 110 in a gaseous phase, and with or without a carrier gas.
The first process material and the second process material are chosen in accordance with the composition and characteristics of a material to be deposited on the substrate. For example, during the deposition of tantalum (Ta) as a barrier layer, the first process material can include a solid film precursor, such as tantalum pentachloride (TaCl5), and the second process material can include a reducing agent, such as hydrogen (H2) gas. In another example, during the deposition of tantalum nitride (TaN) or tantalum carbonitride (TaCN) as a barrier layer, the first process material can include a metal organic film precursor, such as tertiary amyl imido-tris-dimethylamido tantalum (Ta(NC(CH3)2C2H5)(N(CH3)2)3, hereinafter referred to as Taimata®; for additional details, see U.S. Pat. No. 6,593,484), and the second process material can include a reducing agent, such as hydrogen (H2), ammonia (NH3), silane (SiH4), or disilane (Si2H6), or a combination thereof. In another example, when depositing tantalum nitride (i.e., TaNx), the first precursor can include a tantalum-containing precursor, such as TaCl5, PDEAT (pentakis(diethylamido) tantalum), PEMAT (pentakis(ethylmethylamido) tantalum), TaBr5, or TBTDET (t-butylimino tris(diethylamino) tantalum). The second precursor can include a mixture of H2 and N2, or NH3. Still further, when depositing tantalum pentoxide, the first process material can include TaCl5, and the second process material can include H2O, or H2 and O2. Other examples of first and second process material will be provided below with respect to
Additionally, the purge gas supply system 144 can be configured to introduce a purge gas to process chamber 110. For example, the introduction of purge gas may occur between introduction of the first process material and the second process material to process chamber 110, or following the introduction of the second process material to process chamber 110, respectively. The purge gas can comprise an inert gas, such as a Noble gas (i.e., helium, neon, argon, xenon, krypton), or nitrogen, or hydrogen. In one embodiment, the purge gas supply system 144 can also be configured to introduce a reactive purge gas in to chamber 110 as will be further described herein.
The first material supply system 140, the second material supply system 142, and the purge gas supply system 144 can include one or more material sources, one or more pressure control devices, one or more flow control devices, one or more filters, one or more valves, or one or more flow sensors. As discussed with respect to
Referring still to
Referring still to
Optionally, the plasma generation system includes a first electrode in the upper assembly 130, and a second electrode 130A positioned at a periphery of the upper assembly 130 as shown in deposition system 101′ of
Still referring to
Furthermore, the process chamber 110 is further coupled to a pressure control system 132, including a vacuum pumping system 134 and a valve 136, through a duct 138, wherein the pressure control system 134 is configured to controllably evacuate the process chamber 110 to a pressure suitable for forming the thin film on substrate 125, and suitable for use of the first and second process materials. As seen in
Referring now to
While
As discussed in the Related Art section above, one impediment to wide acceptance of ALD processes has been the relatively slow deposition rate of such processes. In particular, conventional ALD processes typically require a cycle of approximately 15-20 seconds to deposit a single layer of material, with the reduction reaction typically accounting for approximately 10 seconds of the cycle time. The present inventors have studied the process parameters of conventional ALD processes in an effort to reduce this deposition time (or improve the deposition rate). As a consequence, the present inventors have determined that the conventional plasma power of 600 W or less may be increased to accelerate the reduction reaction time. For example, in performing a PEALD process such as that described in
For instance, process parameters are provided in Table 1 for an exemplary PEALD process for forming a thin film of tantalum (Ta) using tantalum pentachloride as the first process material and hydrogen as the second process material during the reduction step.
Table 1 provides columns including, from left to right, the ALD process step, the temperature set for the evaporation system configured to sublime the first process material, TaCl5, the flow rate of Ar (carrier Ar, sccm) passing through the evaporation system, the flow rate of hydrogen (H2 sccm) during the reduction step, the flow rate of Ar (Ar, sccm) coupled directly to the process chamber, the time for each step, the power applied during each step, and the pressure set for each step. Additionally, the tantalum film is formed on a silicon dioxide (SiO2) substrate using 300 cycles as described in Table 1, while the temperature of the substrate is set to approximately 240 degrees C.
In
In
Thus, the present inventors have discovered that increasing the plasma power over the conventional limit of approximately 600 W can improve the deposition rate of ALD films, as well as film characteristics such as film resistivity. Moreover, the present inventors have recognized that the use of such a relatively high plasma power provides a more complete release of byproducts from the first process material layer on the substrate, during the reduction reaction when the second process material is introduced to the chamber. Returning to the example above, where tantalum pentachloride is first adsorbed onto the substrate surface, a hydrogen plasma generated at approximately 1000 W will release more chlorine from the tantalum pentachloride layer than a plasma generated at 600 W. For example,
For instance, one explanation for the reduced reduction reaction time at higher plasma power is that the increased power provides a higher density of radicals in the plasma, such as H+ in a hydrogen plasma, that can react with the first precursor on the substrate surface. The availability of more radicals provides for a shorter saturation time in the reduction reaction.
Furthermore, for instance, according to another explanation, reduction on the surface can depend on the surface temperature and, hence, the reduction process should depend on temperature according the Arrhenius relation, i.e., R≅R0 exp(−Eactivation/kTsurface). It is known that plasma produces an apparently lower activation energy than the activation energy in an electrically neutral gas environment. The mechanism for reduced activation energy is caused by ion-neutral interactions, rather than neutral-neutral interaction. Due to reduced apparent activation energy, more reaction products are generated in time, or saturation occurs sooner.
For example, one interpretation is that an increase in plasma power generates a greater reduction in activation energy, whereas less plasma power generates less reduction or zero change in the activation energy. Assuming that for a first plasma power (P1), the amount of released chlorine (Cl) in time interval (Δt) from tantalum pentachloride (TaCl5) by hydrogen radicals (He) is proportional to the reactant(s) density and to the rate constant with Arrhenius dependence on the temperature, that is
ΔnCl(P1)=R0(P1)×nH(P1)×nTaCl
At a second plasma power (P2), such that (P2>P1), the released amount of (Cl) is proportional to
ΔnCl(P2)=R0(P2)×nH(P2)×nTaCl
Based on the assumption that (E2A<E1A) at (P2>P1), and considering (E2A=αE1A) where (α≦1), we can rewrite both relations in a form (considering the same time interval)
ΔnCl(P1,2)=R0 exp(−E1,2A/kT1,2)×nH(P1,2)×nTaCl
Now the ratio of released (Cl) densities for both cases becomes
e.g.
Deconvolution of the last relation into a Taylor series expansion leads to
The ratio,
is always larger than unity, assuming a monotonic increase in hydrogen radicals with plasma power, e.g., k1≧1. Neglecting higher orders in a sum of infinite series, leaving only the first two members,
we can see that
(always) for any values of (0<α≦1), and therefore
From the last estimates we can achieve
that there is always larger amount of chlorine released by hydrogen radicals in the same time interval at higher power, e.g., ΔnCl(P2)≧ΔnCl(P1).
Further yet, for instance, according to another explanation, plasma interaction with the substrate surface can have an effect on the effective surface temperature of the substrate due to ion bombardment. Increased plasma power generates a higher Vpp (peak-to-peak voltage) on the electrode (such as an electrode in the upper assembly 30, or 130), which can cause a higher energy for ions incident on the substrate. Higher energy collisions with the substrate surface can generate a higher effective surface temperature and accelerates surface reactions. With time, local temperature is increased, thus saturation occurs sooner.
In step 430, the second process material is provided in the process chamber to provide a reduction reaction with the deposited first process material in order to form a desired film on the substrate surface. As would be understood by one of ordinary skill in the art, the first and second process materials are selected in accordance with a desired film to be deposited on the substrate. For example, first and second process materials for depositing a tantalum-containing film may include any combination of the tantalum deposition materials discussed above and the reducing agents discussed above.
In one example, when depositing tantalum (Ta), tantalum nitride, or tantalum carbonitride, the first process material can include TaF5, TaCl5, TaBr5, Tal5, Ta(CO)5, Ta[N(C2H5CH3)]5 (PEMAT), Ta[N(CH3)2]5 (PDMAT), Ta[N(C2H5)2]5 (PDEAT), Ta(NC(CH3)3)(N(C2H5)2)3 (TBTDET), Ta(NC2H5)(N(C2H5)2)3, Ta(NC(CH3)2C2H5)(N(CH3)2)3, or Ta(NC(CH3)3)(N(CH3)2)3, and the second process material can include H2, NH3, N2 and H2, N2H4, NH(CH3)2, or N2H3CH3.
In another example, when depositing titanium (Ti), titanium nitride, or titanium carbonitride, the first process material can include TiF4, TiCl4, TiBr4, Til4, Ti[N(C2H5CH3)]4 (TEMAT), Ti[N(CH3)2]4 (TDMAT), or Ti[N(C2H5)2]4 (TDEAT), and the second process material can include H2, NH3, N2 and H2, N2H4, NH(CH3)2, or N2H3CH3.
As another example, when depositing tungsten (W), tungsten nitride, or tungsten carbonitride, the first process material can include WF6, or W(CO)6, and the second process material can include H2, NH3, N2 and H2, N2H4, NH(CH3)2, or N2H3CH3.
In another example, when depositing molybdenum (Mo), the first process material can include molybdenum hexafluoride (MoF6), and the second process material can include H2.
When depositing copper, the first process material can include organometallic compounds, such as Cu(TMVS)(hfac), also known by the trade name CupraSelect®, available from Schumacher, a unit of Air Products and Chemicals, Inc., 1969 Palomar Oaks Way, Carlsbad, Calif. 92009), or inorganic compounds, such as CuCl. The second process material can include at least one of H2, O2, N2, NH3, or H2O. As used herein, the term “at least one of A, B, C, . . . or X” refers to any one of the listed elements or any combination of more than one of the listed elements.
In another example, when depositing ZrO2, the first process material can include Zr(NO3)4, or ZrCl4, and the second process material can include H2O.
When depositing HfO2, the first process material can include Hf(OBut)4, Hf(NO3)4, or HfCl4, and the second process material can include H2O. In another example, when depositing hafnium (Hf), the first process material can include HfCl4, and the second process material can include H2.
In still another example, when depositing niobium (Nb), the first process material can include niobium pentachloride (NbCl5), and the second process material can include H2.
In another example, when depositing zinc (Zn), the first process material can include zinc dichloride (ZnCl2), and the second process material can include H2.
In another example, when depositing SiO2, the first process material can include Si(OC2H5)4, SiH2Cl2, SiCl4, or Si(NO3)4, and the second process material can include H2O or O2. In another example, when depositing silicon nitride, the first process material can include SiCl4, or SiH2Cl2, and the second process material can include NH3, or N2 and H2. In another example, when depositing TiN, the first process material can include titanium nitrate (Ti(NO3)), and the second process material can include NH3.
In another example, when depositing aluminum, the first process material can include aluminum chloride (Al2Cl6), or trimethylaluminum (Al(CH3)3), and the second process material can include H2. When depositing aluminum nitride, the first process material can include aluminum trichloride, or trimethylaluminum, and the second process material can include NH3, or N2 and H2. In another example, when depositing aluminum oxide, the first process material can include aluminum chloride, or trimethylaluminum, and the second process material can include H2O, or O2 and H2.
In another example, when depositing GaN, the first process material can include gallium nitrate (Ga(NO3)3), or trimethylgallium (Ga(CH3)3), and the second process material can include NH3.
Referring again to
The reduction reaction completed by step 440 results in a thin layer of the desired film being deposited on the substrate surface. For example, the reduction reaction may result in a thin layer of a barrier layer, a seed layer, an adhesion layer, a gate layer, a metal layer, a metal oxide layer, a metal nitride layer, or a dielectric layer being deposited on a feature of the substrate. Once the reduction reaction takes place, steps 420-440 of
While not shown in
In addition to the effect of a high plasma power level on the deposition of ALD films, the present inventors have considered the potential effect of relatively low plasma power on the deposition of ALD films. In doing so, the present inventors have determined that a low power plasma may provide for the removal of residual contaminants in the process chamber and the substrate, prior to the actual reduction reaction taking place. Specifically, introduction of the first process material (the film precursor) typically results in this material being adsorbed on the process chamber components, such as the chamber walls, as well as on the substrate. Further, byproducts of previous reduction reactions may exist on the process chamber components. For example, when depositing a tantalum-containing film as described above, residual chlorine from the first process material is typically present on the substrate and chamber components.
During the ALD process, and in particular the plasma-enhanced reduction reaction, materials on the chamber components can be sputtered and can contaminate the deposited film, which can result in a film having poor properties. The present inventors have recognized that although a higher plasma power can lead to a greater deposition rate, reduced film resistivity, and reduced chlorine content in the film (for a chlorine-containing precursor), it can also lead to the appearance of other contaminants in the film arising from the sputtering of process chamber components by large ionized contaminants, such as ionized chlorine (as opposed to the smaller hydrogen ions in a hydrogen plasma reduction step). For instance, when TaCl5 is reduced on the substrate surface using a hydrogen plasma, HCl evolves from the surface, which in the presence of the plasma, dissociates to form ionized chlorine, etc., which is a large ion and capable of sputtering process chamber components. As the plasma power is increased, the sheath voltage adjacent process chamber components can exceed the sputtering threshold for the material composition of the process chamber component. For example, the electrode in the upper assembly 30, 130, as depicted in
Based on the above recognition of the benefits of using low and high power plasmas, the present inventors discovered that varying the plasma power level during an ALD process can provide the dual advantage of reduced contamination of the ALD film as well as improved deposition rate of the film.
In step 540 of
In step 550, a second level of power higher than the first level is coupled to the process chamber to generate a plasma for facilitating a reduction reaction on the substrate surface. Thus, the second level of power should be coupled to the process chamber during introduction of the second process material, but may also be coupled at other times during the ALD process. As with the first power level, the second level of power is largely dependent on the first and second process materials, as well as the time in the ALD process that the second power level is applied. In an embodiment, the second level of power is above 600 W to accelerate the reduction reaction and reduce impurities as described above. However, in the embodiments of
As would be understood by one of ordinary skill in the art, the power curves of
As noted above, varying plasma power such as that shown in the curves 610 and 650 of
In another embodiment, the varying power can occur during other steps in the ALD cycle and serve dual functions. For example, a first power level can be applied during introduction of the first process material to assist in adsorption of the first material to the substrate surface, while also operating to release contaminants from the process chamber. A second power level may also be applied during introduction of the second process material and/or a purge gas step to reduce contaminants. Ultimately, the plasma power level is increased to above 600 W during introduction of the second process material in order to accelerate the reduction process and reduce contamination in the deposited layer as discussed above.
As discussed above, in one embodiment of the present invention an inert purge gas can be introduced into the process chamber during the ALD process. Specifically, as shown in
In step 740, a plasma is generated in the process chamber by coupling electromagnetic power to the process chamber during introduction of the second processing material. The power level coupled to the chamber in step 740 is preferably above 600 W, and, for example, can be about 1000 W in order to accelerate the reduction reaction and reduce contaminants as described above. Moreover, a varying power may be coupled to the process chamber in order to provide further reduction of contaminants as described in
In step 750, a reactive cleaning gas is introduced into the process chamber. Unlike the inert purge gas steps discussed with respect to
In another embodiment, the process chamber walls may be heated in order to facilitate a chemical reaction to remove the contaminants. For example, when reducing chlorine contaminants as described above, the chamber walls are heated to at least 80 degrees C. In some instances, a plasma may also be generated to facilitate the chemical cleaning reaction. However, such plasma should not cause an undesirable reaction at the substrate surface. Once the purge step 750 is completed, the process steps 720 to 750 can be repeated to obtain a desired film thickness as shown by process arrow 760. While
In another embodiment of the present invention, contaminants that affect the ALD process can be reduced by attracting the contaminants away from a substrate region to a peripheral region of the process chamber. Specifically, generation of a plasma within the substrate region ionizes contaminants that can have a detrimental effect on the film deposited on the substrate. For example, when depositing a tantalum-containing material as discussed above, chlorine contaminants in the process chamber are ionized by application of plasma power. As such, the present inventors discovered that generating a separate plasma in a peripheral region of the process chamber can create a potential difference that induces a transport of electrically charged material which removes ionized contaminants from the substrate region to a peripheral region of the process chamber. The attracted contaminants are then either adhered to the process chamber walls or expelled from the process chamber by vacuum pumping, thereby reducing the effects of the contaminants on the deposited film.
As described above, when depositing a tantalum film using tantalum pentachloride as a film precursor (first process material) and hydrogen as a reducing agent (second process material), HCl evolves from the film as a product of the surface reduction reaction. HCl in the presence of the plasma is dissociated, and chlorine ions (Cl−) can be formed. In an electronegative (Cl) plasma, the decay of the electronegative plasma (typical for chlorine) following the shutdown of plasma power is such that the electrons decay quickly due to their high mobility. In a weakly electronegative plasma the negative ions will gradually decay within the substrate zone (A) (see
In other words, during the plasma decay, there are two stages: (1) In the first stage, the flux of negative ions to the wall is absent and the electron density decays sharply with time, whereby almost all electrons escape within a finite time from the discharge volume where an ion-ion (electron-free) plasma is formed, and (2) In the second stage, this plasma decays by an ion-ion ambipolar diffusion mechanism. To provide transport of the ions from the substrate zone (A) towards a peripheral zone (B) (see
For example, both plasma regions can be powered by generating plasma in manner of an overlapping timing sequence. Physical adsorption of chlorine (more generally, reactive products) does not occur within substrate zone (A) when plasma is on in substrate zone (A). Before the turning the plasma off in the substrate zone (A), the plasma in the peripheral zone (B) is initiated. Once the plasma is initiated in the peripheral zone (B), the plasma in the substrate zone (A) is extinguished and ions from the substrate zone (A) are transported to peripheral zone (B), where there is higher probability to be pumped out. This cycling can be repeatedly applied to an electrode in the upper assembly 30 and electrode 30A in
As previously discussed,
The first plasma region in substrate zone (A) can be formed by the plasma source utilized by PEALD process, such as upper assembly (electrode) 30 in FIG. 1A or upper assembly (electrode) 130 in
Dimensionally the secondary plasma electrode (30A, 130A) can coincide approximately with the process chamber dimensions, and have minimal dimensions consistent with the edge of the substrate. Because this electrode assists plasma transport from the substrate zone (A) to the peripheral zone (B), a sufficient cross-section for gas flow has to be provided so as to not restrict pumping speed. Examples of electrode geometry are shown in
Each electrode can be biased by an external power source, such as a radio frequency (RF) power generator through a matching network in a frequency range from 100 kHz to 100 MHz. A pulsed direct current (DC) signal (positive or negative polarity, depending upon the electropolarity of the residual gas) can be used, for example, during the operation of the first plasma source in substrate zone (A) (i.e., electrode 30, or 130 in
Alternatively, the secondary plasma source can include inductively coupled devices to supply electromagnetic power to the peripheral zone (B), such as those inductive devices described in for example, such as described in pending U.S. patent application Ser. No. 10/717,268, attorney docket no. USP03Z003, entitled “Plasma Processing System with Locally-Efficient Inductive Plasma Coupling”.
Other examples of inductive devices include the inductive devices depicted in
In step 840, electromagnetic power is coupled to the process chamber during introduction of the second process material in order to facilitate a reduction reaction as discussed above. In the embodiment of
In step 850, power is coupled to the process chamber to generate a plasma for ionizing contaminants in the region of the substrate as described above. In an embodiment, step 850 of ionizing contaminants is performed as a consequence of generating a reduction reaction in step 840. That is, the process of generating a plasma in step 840 can naturally ionize contaminants in the substrate region thereby simultaneously performing step 850. In alternate embodiments, however, the process step for ionizing the contaminants can be performed independently of the reduction reaction step. For example, process conditioning such as plasma power, chamber environment and chamber pressure may be adjusted from the reduction plasma step in order to provide ideal ionization for the contaminants.
In step 860, power is coupled to a peripheral electrode such as the electrode 30A or the electrode 130A of
For instance, a plasma potential can be established according the highest (positive) potential at a significant surface area interfacing with the plasma boundary. Because the electrically biased surfaces in a PEALD system are the substrate electrode (20/120 in
The peripheral plasma generation step 860 at least partially overlaps the substrate region plasma generation step 850 (as described above; see
As noted above, the plasma in the substrate zone (A) and the peripheral zone (B) can be generated independently of the plasma generation step 840 for reduction reaction. In addition, while not shown in
In yet another embodiment of the present invention, contaminants that affect the ALD process can be removed from the process chamber by vacuum pumping the chamber through gas injection orifices of a gas injection assembly. Specifically, the present inventors have recognized that during generation of a plasma within the processing system, power applied to a gas injection assembly causes the plurality of gas injection orifices to act as “hollow anodes” that attract species of the plasma including ionized contaminants. For example, when depositing tantalum-containing material as discussed above, chlorine contaminants in the process chamber can be ionized and attracted to hollow anodes of a gas injection assembly. The present inventors discovered that vacuum pumping the plurality of orifices during plasma generation can reduce the contaminants within the process chamber, thereby reducing the effects of the contaminants on the deposited film.
As previously discussed,
In the embodiment shown in
In step 940, electromagnetic power is coupled to the process chamber during introduction of the second process material in order to facilitate a reduction reaction. In the embodiment of
In step 950, power is applied to a gas injection electrode to generate a plasma for ionizing contaminants in the process chamber. The power applied to the gas injection electrode biases the electrode so that gas injection orifices also act as hollow anodes in step 950 to attract the ionized contaminants as discussed above. In an embodiment, step 950 of ionizing contaminants is performed as a consequence of generating the reduction reaction plasma in step 940. That is, the process of applying power to the gas injection electrode to generate a reduction reaction plasma in step 940 can naturally ionize contaminants and create hollow anodes thereby simultaneously performing step 950. In alternate embodiments, however, the process step for ionizing and attracting contaminants can be performed independently of the reduction reaction step.
In step 960, the ionized contaminants are vacuum pumped from the process chamber through a plurality of orifices in the gas injection electrode. The vacuum pumping step 960 at least partially overlaps the plasma generation step 950 in order to expel the ionized contaminants as discussed above. Thus, in an embodiment where ionizing the contaminants results from the reduction reaction plasma, steps 930, 940, 950 and 960 of
While not shown in
For example, in one embodiment, the first process material may be introduced in step 920 by gas injection orifices on the gas injection electrode. Then, in step 930, the second process material is introduced using a separate gas injection path while power is applied to the gas injection electrode in step 940 to generate a reduction reaction plasma. The alternative gas injection path may be, for example, the sidewall gas injection valve discussed in
As discussed above, various techniques may be employed within a PEALD processing system to remove contaminants such as chlorine from the processing system and/or a substrate processed in the PEALD system. The present inventors have recognized, however, that despite these efforts, contaminants can deposit on the ALD film during transfer of the substrate from the PEALD process chamber to a separate process chamber for further processing, such as interconnect metallization. The inventors have observed that the sheet resistance, after a 400 degrees C. anneal, of film structures consisting of an approximately 10 nm thick Cu layer, upon an approximately 6 nm thick layer of tantalum, upon an approximately 6 nm thick layer of tantalum nitride exhibits a significant increase when the tantalum layer is prepared with a PEALD process utilizing tantalum pentachloride as the film precursor. In this film structure, the Cu and tantalum nitride films are prepared using ionized PVD (i-PVD). For example, when the tantalum film is prepared using i-PVD, the sheet resistance is approximately 8.04 ohms/square and, when the tantalum film is prepared using PEALD (as described above), the sheet resistance is approximately 145 to 185 ohms/square and metal (copper) agglomeration is observed.
The present inventors have also recognized that the above described transfer contamination problems can occur for films deposited by non-plasma ALD, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), or any other deposition process. That is, despite efforts to reduce contamination within the deposition chamber itself, contaminants can affect the deposited film during transfer of the substrate from the deposition process chamber to a separate process chamber for further processing, such as interconnect metallization.
Thus, despite cleaning efforts in a PEALD or other deposition chamber, metallization can be deposited on a contaminated ALD or other deposited film, leading to operation and reliability problems in the end device. Based on this recognition, the present inventors have discovered that contaminants can be further reduced on the substrate by performing a plasma cleaning of the substrate after the substrate is removed from the deposition system.
After completion of the deposition process, the substrate having the ALD film deposited thereon is transferred to a treatment chamber where a plasma cleaning is performed as shown by step 1030. The plasma cleaning is preferably performed with a plasma characterized by low electron temperature (less than about 1.5 eV) and high plasma density (>1×1012/cm3), that enables substantially damage-free cleaning of the deposited layer according to the invention. Such process parameters create a “soft plasma” that effectively reduces contaminants on the substrate surface (i.e., the deposited film such as an ALD film surface) without substantially damaging the deposited film. In step 1040, further processing is performed on the substrate. For example, step 1040 may include deposition of interconnect metallization on the deposited film.
In one embodiment of the invention, the plasma cleaning step 1030 is performed in a designated treatment chamber, and then transferred to an additional process chamber for performing processing step 1040. For example, the treatment chamber includes a slotted plane antenna (SPA) plasma source which will be described below.
In another embodiment, the plasma cleaning step 1030 is performed in the same chamber as the processing step 1040. For example, where processing step 1040 is a metallization step performed in an ionized physical vapor deposition (i-PVD) chamber, the plasma cleaning step 1030 can be performed in the i-PVD chamber prior to depositing the metal. Specifically, the i-IPVD process can be provided by an apparatus for sputtering conductive metal coating material from an annular magnetron sputtering target. Sputtering can be accomplished by applying a DC power to the target and the sputtered material is ionized in a processing space between a target and a substrate by generating a dense plasma in the space. The ionized sputter material is then drawn to the substrate surface by applying a bias to the substrate. Where the plasma cleaning step is performed in the i-PVD chamber, the substrate having an deposited film thereon is first exposed to an inert gas such as argon in the i-PVD chamber. Power is coupled to the i-PVD chamber to heat the inert gas and generate a plasma for reducing contaminants on the substrate surface, as described above. During the plasma cleaning treatment of the substrate, no power is coupled to the metal target, and the use of substrate bias power is optional. Once the cleaning step is completed, DC power to the metal target and substrate bias power is applied to perform the i-IPVD metallization process. The inventors have observed that the sheet resistance after 400° C. anneal of film structures consisting of an approximately 10 nm thick Cu layer, upon an approximately 6 nm thick layer of tantalum, upon an approximately 6 nm thick layer of tantalum nitride exhibits no increase when the tantalum layer is prepared with a PEALD process utilizing tantalum pentachloride as the film precursor and the plasma cleaning is performed. In addition, no copper agglomeration is observed.
In the embodiment of
In the plasma processing system 1250, microwave power is provided to the process chamber 1250 through the top plate 1254 via a plane antenna member 1260 having a plurality of slots 1260A. The slot plane antenna 1260 can be made from a metal plate, for example copper. In order to supply the microwave power to the slot plane antenna 1260, a waveguide 1263 is disposed on the top plate 1254, where the waveguide 1263 is connected to a microwave power supply 1261 for generating microwaves with a frequency of 2.45 GHz, for example. The waveguide 1263 contains a flat circular waveguide 1263A with a lower end connected to the slot plane antenna 1260, a circular (coaxial) waveguide 1263B connected to the upper surface side of the circular waveguide 1263A, and an outport (bottom surface in
Inside the circular waveguide 1263B, an axial portion 1262 (or inner conductor) of an electro-conductive material is coaxially provided, so that one end of the axial portion 1262 is connected to the central (or nearly central) portion of the upper surface of slot plane antenna 1260, and the other end of the axial portion 1262 is connected to the upper surface of the circular waveguide 1263B, thereby forming a coaxial structure. As a result, the circular waveguide 1263B is constituted so as to function as a coaxial waveguide. The microwave power can, for example, be between about 0.5 W/cm2 and about 4 W/cm2. Alternately, the microwave power can be between about 0.5 W/cm2 and about 3 W/cm2.
In addition, in the vacuum process chamber 1250, a substrate holder 1252 is provided opposite the top plate 1254 for supporting and heating a substrate 1258 (e.g., a wafer). The substrate holder 1252 contains a heater 1257 to heat the substrate 1258, where the heater 1257 can be a resistive heater. Alternately, the heater 1257 may be a lamp heater or any other type of heater. Furthermore the process chamber 1250 contains an exhaust line 1253 connected to the bottom portion of the process chamber 1250 and to a vacuum pump 1255.
Still referring to
Although only certain exemplary embodiments of inventions have been described in detail above, those skilled in the art will readily appreciate that many modifications are possible in the exemplary embodiments without materially departing from the novel teachings and advantages of this invention. For example, various techniques have been disclosed herein for improving ALD cycle times and reducing contamination of ALD films. Any combination or all of these features can be implemented in a single ALD processing system. Accordingly, all such modifications are intended to be included within the scope of this invention.